Cold heading wire: processes and delivery conditions

Read process sequences and delivery conditions by standard system. Confirm grade, product form, edition and acceptance requirements together.

Purpose of each operation

Wire rod and traceability

Verify grade, heat, size and certificates; retain traceability through processing.

Pickling

Remove scale and prepare the surface for subsequent treatment or coating.

Spheroidize annealing

Improve carbide form and ductility where applicable; distinguish ordinary annealing and solution treatment.

Surface treatment and phosphating

Provide a suitable lubricant carrier; pickling, phosphating and lubrication are distinct operations.

Cold and light drawing

Control size and section through dies; final light drawing differs from substantial cold reduction.

Inspection

Check size, surface and ordered properties; record spheroidization and decarburization where required.

Packaging

Protect wire from corrosion, handling damage and mixing of heats during transport.

Dispatch

Check labels, heats, quantities and documents, retaining dispatch traceability.

China · GB

GB/T 5953.1-2009 §3.2 · GB/T 5953.2-2009 §3 · GB/T 5953.3-2012 §3 · GB/T 5953-2026

HD is cold drawn; SA adds spheroidizing after drawing; SALD adds final light drawing; ASALD adds an earlier anneal. GB/T 5953.1-2009 covers four conditions, while Part 2 covers HD and SALD. GB/T 5953-2026 takes effect on 1 December 2026. Specify the edition in the order. GB/T 5953.3-2012: HD. GB/T 6478: Bar / Wire rod. GB/T 28906: Wire rod.

HD
Cold drawing
GB/T 5953.1; Part 2 covers HD and SALD
SA
Cold drawingSpheroidize annealing
GB/T 5953.1; Part 2 covers HD and SALD
SALD
Cold drawingSpheroidize annealingLight drawing / skin passing
GB/T 5953.1; Part 2 covers HD and SALD
ASALD
AnnealingCold drawingSpheroidize annealingLight drawing / skin passing
GB/T 5953.1; Part 2 covers HD and SALD

China · GB →

Japan · JIS

JIS G 3507-2:2005 Table 1 (3), §5 · JIS G 3508-2:2005 · JIS G 3509-2:2003

DA includes cold working, annealing and final cold working, or annealing of rod followed by cold working. It does not by itself require spheroidizing. Confirm commercial AD/DAD notation operation by operation. R/A/K in SWCH grades describe deoxidation, separately from D/DA processing. Check the boron and low-alloy wire standards G 3508-2 and G 3509-2 separately.

D
Wire rodCold drawing
JIS G 3507-2 Table 1, note (3)
DA
Wire rodCold drawingAnnealingCold drawing
JIS G 3507-2 Table 1, note (3)
DA
Wire rodAnnealingCold drawing
JIS G 3507-2 Table 1, note (3)
D · G 3508-2
Wire rodCold drawing
JIS G 3508-2:2005 · Table 1 (2) · SWCHB223 / 320 / 420 / 526 / 620
DA · G 3508-2
Wire rodCold drawingAnnealingCold drawing
JIS G 3508-2:2005 · Table 1 (2)
DA · G 3508-2
Wire rodAnnealingCold drawing
JIS G 3508-2:2005 · Table 1 (2)
DA1 · G 3509-2
AnnealingCold drawing
JIS G 3509-2:2003 §3, Table 1 (3)
DA2 · G 3509-2
Cold drawingAnnealingCold drawing
JIS G 3509-2:2003 §3, Table 1 (3)
DA3 · G 3509-2
AnnealingCold drawingAnnealingCold drawing
JIS G 3509-2:2003 §3, Table 1 (3)

Japan · JIS →

United States · ASTM

ASTM F2282-23 §3.1.10, §3.1.10.1/.2, §5.5.1

DFAR/DFAB are drawn from annealed rod/bar; DFSR/DFSB use spheroidize-annealed feedstock. SAFS is spheroidized after final drawing. AIP and SAIP are annealed or spheroidized before final light drawing. Cleaning and coating are separate operations. CHQ, AK and FG describe cold-heading quality, aluminium killing and fine grain, rather than a heat-treatment route.

DD
Wire rodCold drawing
ASTM F2282-23
DFAR / DFAB
Annealed rod / barCold drawing
ASTM F2282-23
DFSR / DFSB
Spheroidize-annealed rod / barCold drawing
ASTM F2282-23
SAFS
Drawing to finished sizeSpheroidize annealing
ASTM F2282-23
AIP
Cold drawingAnnealingCleaning and coatingLight drawing / skin passing
ASTM F2282-23
SAIP
Cold drawingSpheroidize annealingCleaning and coatingLight drawing / skin passing
ASTM F2282-23

United States · ASTM →

Europe · EN / historical DIN

EN 10263-2/-3/-4/-5:2017 · DIN 1654:1989 (historical)

Keep +AC, +C and +LC distinct: spheroidizing, drawing and light drawing. +AC+C does not necessarily mean light drawing. Apply Parts 2, 3, 4 and 5 to their respective steel families and product forms; +FP is a bar condition. Stainless +AT solution treatment differs from +A soft annealing. +H, +HH, +HL and +CH concern hardenability or core hardening, not an annealing sequence.

+U
Hot rolling
EN 10263-2 Table 1: wire rod, bar
+U+PE
Hot rollingPeeling
EN 10263-2 Table 1: wire rod, bar
+U+C
Hot rollingCold drawing
EN 10263-2 Table 1: bar, wire
+U+C+AC
Hot rollingCold drawingSpheroidize annealing
EN 10263-2 Table 1: bar, wire
+U+C+AC+LC
Hot rollingCold drawingSpheroidize annealingLight drawing / skin passing
EN 10263-2 Table 1: bar, wire
+AC
Spheroidize annealing
EN 10263-2 Table 1: wire rod, bar
+AC+PE
Spheroidize annealingPeeling
EN 10263-2 Table 1: wire rod, bar
+AC+C
Spheroidize annealingCold drawing
EN 10263-2 Table 1: bar, wire
+U
Untreated
EN 10263-3 Table 1: wire rod, bar, wire
+AC
Spheroidize annealing
EN 10263-3 Table 1: wire rod, bar, wire
+FP
Controlled ferrite-pearlite structure and hardness
EN 10263-3 Table 1: bars only
+U
Untreated
EN 10263-4 Table 1: wire rod, bar
+AC
Spheroidize annealing
EN 10263-4 Table 1: wire rod, bar, wire
+A
Soft annealing
EN 10263-5 Table 1: ferritic and martensitic stainless steels; wire rod, bar, wire
+AT
Solution treatment
EN 10263-5 Table 1: austenitic and duplex stainless steels; wire rod, bar, wire
+C
Cold drawing
EN 10263-5 Table 2: wire rod, wire
+PE
Peeling
EN 10263-5Table2: Bars, Wire
+LC
Light drawing / skin passing
EN 10263-5Table2: Wire Only

Europe · EN / historical DIN →

Other customer specifications

The following are examples of process requirements in other customer specifications. The order and technical agreement accepted by both parties govern the actual sequence. Shared terms such as SAIP retain their meaning under the applicable national or international standard; these examples do not establish a universal delivery specification.

HD · W/R–PC–SKP–CP
Wire rodPickling and specified surface treatmentLight drawing / skin passingPackaging
Example process agreement
S)AIP · W/R–PC–SA–PC–SKP–CP
Wire rodPickling and specified surface treatmentSpheroidize annealingPickling and specified surface treatmentLight drawing / skin passingPackaging
Example process agreement
SAIP · W/R–PC–WD–SA–PC–SKP–CP
Wire rodPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentLight drawing / skin passingPackaging
Example process agreement
PASAIP · W/R–LA–PC–WD–SA–PC–SKP–CP
Wire rodLow-temperature annealingPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentLight drawing / skin passingPackaging
Example process agreement
PSASAIP · W/R–PC–SA–PC–WD–SA–PC–SKP–CP
Wire rodPickling and specified surface treatmentSpheroidize annealingPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentLight drawing / skin passingPackaging
Example process agreement
W/R
Wire rod
Example process agreement
PC · Pickling & Coating
Pickling and specified surface treatment
Example process agreement
WD · Wire Drawing
Cold drawing
Example process agreement
SKP · Skin Pass
Light drawing / skin passing
Example process agreement
LA · Low Temperature Annealing
Low-temperature annealing
Example process agreement
RA · Regular Annealing
Annealing
Example process agreement
SA · Spheroidized Annealing
Spheroidize annealing
Example process agreement
CP · Coil Packing
Packaging
Example process agreement

Heat Treatment and Delivery Conditions

The following explains all 29 treatment-condition symbols in Table 18 of EN 10027-1:2016. Check the general meaning, the delivery conditions permitted by the relevant product standard and the actual processing sequence separately. These symbols do not all apply to cold-heading wire and do not define our supply capability.

EN 10027-1:2016 · Table 18

+A
Soft annealing to reduce hardness and improve subsequent processing.
+AC
Spheroidizing annealing: A process that transforms carbides in applicable steels into a spheroidal form.
+AR
As-rolled condition: No special rolling or heat treatment requirements are specified.
+AT
Solution treatment: Solid-solution annealing performed according to the applicable steel grade.
+C
Work-hardened condition: Achieved through cold working; the specific method depends on the product standard.
+Cnnn
Work hardened, with a minimum tensile strength specified as nnn MPa.
+CPnnn
Work hardened, with a minimum 0.2% proof strength specified as nnn MPa.
+CR
Cold-rolled condition.
+DC
The manufacturer selects the delivery condition, but the material must still meet the applicable standards and order requirements.
+FP
Treated to achieve the specified ferrite–pearlite microstructure and hardness range.
+HC
Hot rollingWork-hardened condition: Achieved through cold working; the specific method depends on the product standard.
+I
Isothermal treatment; microstructure and mechanical properties determined according to the relevant standard or technical agreement.
+LC
Skin-pass finishing by temper rolling or light drawing.
+M
Thermomechanical forming condition.
+N
Normalizing or normalized forming condition.
+NT
NormalizingTempering
+P
Precipitation-hardening condition, applicable to corresponding precipitation-hardening steel grades.
+Q
Quenched condition.
+QA
Air quenching.
+QO
Oil quenching.
+QT
QuenchingTempering
+QW
Water quenching.
+RA
Recrystallization annealing.
+S
Treatment to improve cold shearability.
+SR
Stress-relief treatment.
+T
Tempered condition.
+TH
Treated to achieve a specified hardness range.
+U
Not heat-treated; the specific original processing condition is confirmed according to the product standard.
+WW
Warm working condition.

+QT denotes the quenched-and-tempered (QT) condition, +Q indicates quenching only, and +T indicates tempering only; +N refers to normalizing or normalized forming, while +NT denotes normalizing followed by tempering. Materials delivered in the quenched-and-tempered state should be ordered separately from spheroidizing annealed materials supplied for subsequent quenching and tempering.

The objectives of the treatments represented by +A, +AC, +AT, +RA, and +SR differ: they address softening, carbide spheroidization, solid solution treatment, recrystallization, and stress relief, respectively; +I indicates isothermal treatment and does not allow one to infer microstructure or spheroidization rate solely from this symbol.

In this general designation table, +C means cold-work hardened; in product standards such as EN 10263, it denotes cold drawing. +LC means skin-pass finishing by temper rolling or light drawing. Interpret +M, +HC and +WW under the relevant product standard as well.

+Cnnn specifies a minimum tensile strength of nnn MPa; +CPnnn specifies a minimum 0.2% proof strength of nnn MPa. +TH identifies treatment to an agreed hardness range. Specify the values, test method and sampling position; +TH does not mean spheroidizing annealing.

Symbols with identical codes may have different meanings depending on the standard in which they appear. For example, in the EN 10027-1 table 17, +A, +S, and +T denote corresponding coatings, whereas in the 18 table, the same symbols represent treatment conditions. When placing an order, the product standard, steel grade, condition, and acceptance criteria must be specified simultaneously.

Bright steel processing conditions and their sequence

ISO 683-7:2023 and EN ISO 683-7:2024 cover the relevant non-alloy and alloy bright steel products. Their delivery conditions are distinct from those in the cold-heading product standard EN 10263. Check each combination against the applicable steel grade, product form, dimensions and mechanical-property table.

ISO 683-7:2023 · EN ISO 683-7:2024

+C
Cold drawing
+SH
Peeling / turning
+G
Grinding
+PL
Polishing
+C+G
Cold drawingGrinding
+C+PL
Cold drawingPolishing
+QT+SH
QuenchingTemperingPeeling / turning
+C+QT
Cold drawingQuenchingTempering
+QT+C
QuenchingTemperingCold drawing
+A+SH
Soft annealingPeeling / turning
+A+C
Soft annealingCold drawing
+FP+SH
Controlled ferrite-pearlite structure and hardnessPeeling / turning
+FP+C
Controlled ferrite-pearlite structure and hardnessCold drawing
+C+N
Cold drawingNormalizing
+C+A
Cold drawingSoft annealing
+C+FP
Cold drawingControlled ferrite-pearlite structure and hardness
+N+SH
NormalizingPeeling / turning

Hardening requirements and treatment conditions

+H, +HH, +HL and +CH specify hardenability or core-hardening acceptance requirements. They do not mean that the material is delivered in the quenched-and-tempered condition +QT. Check the Jominy end-quench limits, restricted bands, core hardness and applicable diameters under EN 10263-3/-4, clause 6.4, and ISO 4954-1, clause 7.1.4.

+H
Specifies a standard hardenability band; acceptance is based on the corresponding end-quench test hardness requirement.
+HH
Restricted hardenability band with the same upper limit as the corresponding +H band.
+HL
Restricted hardenability band with the same lower limit as the corresponding +H band.
+CH
Specifies core hardening requirements and verifies the corresponding maximum diameter and core hardness.

Process combinations and sequence

These examples explain process sequences. Specify the annealing requirements for LA/RA, whether PC includes phosphating and whether final D is light drawing. Identify SAF separately from ASTM F2282 SAFS, and confirm whether (S) calls for spheroidizing. The applicable standard, steel grade and agreed technical requirements determine the actual route.

HD · PC–D
Pickling and specified surface treatmentCold drawing
RA · PC–RA
Pickling and specified surface treatmentAnnealing
SA · PC–SA
Pickling and specified surface treatmentSpheroidize annealing
RAIP · PC–RA–PC–D
Pickling and specified surface treatmentAnnealingPickling and specified surface treatmentCold drawing
(S)AIP · PC–SA–PC–D
Pickling and specified surface treatmentSpheroidize annealingPickling and specified surface treatmentCold drawing
SAF · PC–D–SA–PC
Pickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatment
SAIP · PC–D–SA–PC–D
Pickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentCold drawing
PASAF · PC–LA–PC–D–SA–PC
Pickling and specified surface treatmentAnnealingPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatment
PASAIP · PC–LA–PC–D–SA–PC–D
Pickling and specified surface treatmentAnnealingPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentCold drawing
PSASAIP · PC–SA–PC–D–SA–PC–D
Pickling and specified surface treatmentSpheroidize annealingPickling and specified surface treatmentCold drawingSpheroidize annealingPickling and specified surface treatmentCold drawing
+AT+C
Solution treatmentCold drawing
Stainless steel: applicable structure and table
+AT+C+AT
Solution treatmentCold drawingSolution treatment
Stainless steel: applicable structure and table
+AT+C+AT+LC
Solution treatmentCold drawingSolution treatmentLight drawing / skin passing
Stainless steel: applicable structure and table
+A+LC
Soft annealingLight drawing / skin passing
Stainless steel: applicable structure and table
+A+C+A
Soft annealingCold drawingSoft annealing
Stainless steel: applicable structure and table
+A+C+A+LC
Soft annealingCold drawingSoft annealingLight drawing / skin passing
Stainless steel: applicable structure and table

DIN and EN process notation

Historical DIN uses K for drawing and GKZ for spheroidizing. These combinations describe sequence; they are not all fixed delivery conditions in current EN standards. Agree repeated +AC+C+AC routes and any final +LC separately. C means drawing; LC explicitly means light drawing.

K
+U+C
K+GKZ
+U+C+AC
GKZ+K
+AC+C
K+GKZ+K
+U+C+AC+LC
GKZ+K+GKZ
+AC+C+AC
GKZ+K+GKZ+K
+AC+C+AC+LC

International and other national standards

ISO 4954-1:2024 covers non-alloy and alloy steels; ISO 4954-2:2024 covers stainless steels. They replace ISO 4954:2022. Apply KS, CNS, IS and GOST to the specified product form and relevant product standard. GOST 10702 concerns bars for cold bulk forming. National EN prefixes identify national adoptions of the same European standard.

ISO 4954-1:2024 §6.3.2 · Table 1

+AR
As-rolled surface
Bar / Wire rod
+C
Cold drawing
Bar / Wire
+LC
Light drawing / skin passing
Bar / Wire
+PE
Peeling
Bar / Wire rod / Wire

Specify the steel grade and standard edition, finished dimensions and tolerances, surface or coating, mechanical properties, spheroidization and decarburization requirements, inspection documents and heat traceability. Similar codes do not establish material interchangeability. Creation Group processes and supplies cold-heading wire; subsequent part forming and heat treatment are qualified for the customer's process requirements.

Standards and editions

(18)