ISO 4954:2018 Annex A reference scope

Annex A covers steels not intended for heat treatment after cold working. This page reproduces the reviewed 2018 edition’s delivery-condition, cast-analysis and mechanical-property tables. The edition and requirements agreed in the order govern acceptance; these reference excerpts are not a batch certificate or a declaration that every illustrated product complies with this standard.

Creation Group provides cold-heading wire and shaped-wire material processing, testing and technical services through its Shanghai operating team and Wuhu manufacturing base. Confirm grade, product form, delivery condition and application requirements through technical review.

Related catalogue references

The following original catalogue illustrations and linked pages are related references; they do not establish grade equivalence or suitability for a particular component.

Processing illustrations

The original catalogue illustrates wire rod, surface preparation, drawing, annealing, inspection and finished material. Select the actual route for the ordered grade and delivery condition. These photographs do not establish a particular processing cycle, manufacturing history or batch result.

Source-bound technical tables

Use Table A.1 to identify the delivery condition and product form before applying Tables A.2 and A.3. Blank cells, dashes, limits and footnotes retain the distinctions in the reviewed source. Wide tables scroll horizontally on smaller screens.

1. Delivery conditions and applicable requirements

Table A.1 – Heat-treatment conditions, product forms and applicable requirements

Delivery conditionSymbolWire rodBarWire
Untreated, as hot rolled+ARXX—
Untreated and peeled+AR+PEXX—
Untreated and cold drawn+AR+C—XX
Untreated, cold drawn and spheroidize annealed+AR+C+AC—XX
Untreated, cold drawn, spheroidize annealed and skin passed+AR+C+AC+LC—XX
Annealed to achieve spheroidal carbides, as treated or peeled+AC or AC+PEXX—
Annealed to achieve spheroidal carbides, then cold drawn+AC+C—XX

X = applicable; — = not applicable. Chemical composition is specified in Table A.2 and mechanical properties in Table A.3. Supplementary or special requirements under Annex E apply if agreed at enquiry and order. Other delivery conditions may be agreed at the time of order. Source: ISO 4954:2018, Table A.1, page 17 (PDF page 23). The source notation “+AC or AC+PE” is retained as printed; confirm the exact delivery condition in the order.

2. Chemical composition

Table A.2 – Chemical composition by cast analysis of steels not intended for heat treatment after cold working

Steel nameMass fraction, %a
CSiMnPSCrNiMoAlbCuCr + Ni + Mo
C2C0.030.100.20 to 0.40d0.0200.0250.300.300.100.020 to 0.0600.300.50
C4C0.02 to 0.060.100.25 to 0.400.0200.0250.300.300.100.020 to 0.0600.300.50
C8C0.06 to 0.100.100.25 to 0.450.0200.0250.300.300.100.020 to 0.0600.300.50
C10C0.08 to 0.120.100.30 to 0.500.0250.0250.300.300.100.020 to 0.0600.300.50
C10GC0.08 to 0.120.15 to 0.25c0.30 to 0.500.0250.0250.300.300.10—c0.300.50
C15C0.13 to 0.170.100.35 to 0.600.0250.0250.300.300.100.020 to 0.0600.300.50
C15GC0.13 to 0.170.15 to 0.25c0.35 to 0.600.0250.0250.300.300.10—c0.300.50
C17C0.15 to 0.190.100.65 to 0.850.0250.0250.300.300.100.020 to 0.0600.300.50
C17GC0.15 to 0.190.15 to 0.25c0.65 to 0.850.0250.0250.300.300.10—c0.300.50
C20C0.18 to 0.220.100.70 to 0.90d0.0250.0250.300.300.100.020 to 0.0600.300.50
C20GC0.18 to 0.220.15 to 0.25c0.70 to 0.90d0.0250.0250.300.300.10—c0.300.50
C25C0.23 to 0.270.100.80 to 1.00d0.0250.0250.300.300.100.020 to 0.0600.300.50
C25GC0.23 to 0.270.15 to 0.25c0.80 to 1.00d0.0250.0250.300.300.10—c0.300.50

Elements not listed must not be intentionally added to the steel without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions of elements from scrap or other production materials. Residual elements may nevertheless be present if they do not impair mechanical properties or suitability.

a Values are maximum limits unless otherwise indicated.

b Aluminium may be replaced by one or more elements with a similar effect.

c C10GC, C15GC, C17GC and C20GC may be supplied in two qualities: a) with a maximum aluminium content of 0.015%, or b) without aluminium and with silicon of 0.15 to 0.25% for hot-dip galvanizing.

d For C2C, C20C, C20GC and C25C, a lower manganese content may be specified with a range of 0.20%.

Source note: The C25GC row carries footnote markers c and d in ISO 4954:2018, but C25GC is not named in the wording of these footnotes. The markers and notes are reproduced as in the source; the conditions require clarification before application to C25GC.

3. Mechanical properties

Table A.3 – Mechanical properties of wire rod, bars and wire not intended for heat treatment after cold working

Steel nameDiameterDelivery condition
+AR or +AR+PE+AC or +AC+PE+AR+C+AR+C+AC+AR+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZa min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
C2C25——————3108035075——
51036075——450703008034075——
104036075——440703008034075——
4010036075——440683008034075——
C4C25————3207736073——
510390703307547066310773507341070
1040390703307546066300773507340070
401003907033075————————
C8C25——————3507239068——
510410653607049063340723806845065
1040410653607048063340723806844065
401004106536070————————
C10C / C10GC25——————3707241068——
510430603807052058360724006847063
1040430603807051058360724006846063
401004306038070————————
C15C / C15GC25——————3907043066——
510460584006855056380704206649063
1040460584006854056380704206648063
401004605840068————————
C17C / C17GC25——————4306747063——
510520584406561056420674606353060
1040520584406560056420674606352060
401005205844065————————
C20C / C20GC25——————4706751063——
510560554806565053460675006357060
1040560554806564053460675006356060
401005605548065————————
C25C25——————5006554060——
510590505106068050490655306060055
1040590505106067050490655306059055
401005905051060————————
C25GC25————57045——44055——
51059050——47045——4405544055
104059050——47045——4405544055
4010059050——————————
a Values are given for information only.

Reference edition: ISO 4954:2018. These excerpts do not replace the complete standard or a delivery-batch inspection certificate. Annex A supplies no hardenability table for these grades.

Inspection equipment and example images

These original catalogue images illustrate equipment and examination methods. They are not batch certificates or proof that every test is required for every Annex A grade. Magnifications and hardness scales retain the original catalogue labels; confirm the actual method, conditions and calibrated scale in the inspection record.

Delivery and packaging

Delivery options in the catalogue include coils, straight lengths and export wooden crates. Protective options include end-face wooden boards, wrapping, PP woven bags, wire racks and pallets. Confirm the selected arrangement in the order. Packaging illustrations do not establish technical compliance or a verified loading record.