Technical data for ML15 cold heading steel wire rod, compliant with GB/T 5953. View the chemical composition, mechanical properties, and related technical requirements for this grade.
Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.
When determining acid-soluble aluminum Al, Al≥0.015%.
When determining acid-soluble aluminum Al, Al≥0.015%.
2. Mechanical Properties
Table 2 Tensile strength, reduction of area, and hardness of HD process steel wire
2.1 For cold heading wire produced by the HD process, tensile strength and reduction of area shall comply with the requirements specified in Table 2.
Grade a)
Nominal wire diameter d / mm
Tensile strength Rm / (N/mm²)
Reduction of area Z / %
Rockwell hardness b) / HRB
ML15Al ML15
≤3.00
≥590
≥50
—
>3.00~4.00
≥490
≥50
—
>4.00~5.00
≥420
≥50
—
>5.00~25.00
≥400
≥50
<89
Note: For nominal wire diameters greater than 20 mm, the reduction of area may be reduced by 5%.
a) The chemical composition of the grades may refer to GB/T 6478. b) Hardness values are for reference only.
Note: For wire with a nominal diameter greater than 20 mm, the reduction of area may be reduced by 5%. a) The chemical composition of the grades may refer to GB/T 6478. b) Hardness values are for reference only.
Table 3 Tensile strength, reduction of area, and hardness of wire produced by the SALD process
2.2 For cold heading wire produced by the SALD process, the tensile strength and reduction of area shall comply with the requirements specified in Table 3.
Grade a)
Tensile strength Rm/ (N/mm²)
Reduction of area Z / %
Rockwell hardness b) HRB
ML15Al ML15
340〜500
>65
<81
Note: For nominal wire diameters greater than 20 mm, the reduction of area may be reduced by 5%.
a) The chemical composition of the grades may refer to GB/T 6478. b) Hardness values are for reference only.
Note: For wire with a nominal diameter greater than 20 mm, the reduction of area may be reduced by 5%. a) The chemical composition of the grades may refer to GB/T 6478. b) Hardness values are for reference only. 2.3 The mechanical properties of wire with a nominal diameter greater than 25.00 mm shall be determined by agreement between the supplier and the purchaser. 2.4 The mechanical properties of wire grades not listed in the table shall be determined by agreement between the supplier and the purchaser. 2.5 Upsetting Cold heading wire produced by the HD process: Wire samples shall show no cracks or fissures after being cold upset to one-half of their original height. Cold heading wire produced by the SALD process: Wire samples shall show no cracks or fissures after being cold upset to one-third of their original height. No upsetting test is required for wire with a diameter ≤ 5.0 mm.
3. Microstructure
Table 4 Permissible range for decarburized layer depth
Table 4 Permissible range for decarburized layer depth
Unit: mm
Nominal wire diameter/d
Depth of complete decarburization
Total decarburized layer depth
<10.00
≤0.02
≤0.01 d
≥10.00—15.00
≤0.02
≤0.15
≥15.00〜25.00
≤0.03
≤0.20
Note: When the nominal wire diameter exceeds 25.00 mm, the permissible range for decarburized layer depth shall be determined by agreement between the supplier and the purchaser.
6.1 Microstructure For wire produced by the SALD process, the microstructure shall be spheroidized. The spheroidizing grade shall be agreed upon by the supplier and the purchaser and assessed in accordance with JB/T 5074. The test method for the decarburized layer shall be determined by agreement between the supplier and the purchaser. 6.2 Decarburized layer depth Wire produced by the SALD process shall undergo decarburization testing. The permissible ranges for the depth of complete decarburization on one side and the total decarburized layer depth (ferrite + transition layer) shall comply with the provisions of Table 4. The test method for the decarburized layer shall be determined by agreement between the supplier and the purchaser. 6.3 Carburization Wire produced by the SALD process shall not exhibit surface carburization. Testing may be omitted if guaranteed by the supplier.
4. Comparison table of non-heat-treated cold heading steel grades with domestic and international equivalents; see Table B.1 for grade comparisons.
Table B.1 Cross-reference of non-heat-treated cold heading steel grades with domestic and international equivalents
Unified digital code
This standard
GB/T 6478
ISO 4954
EN 10263-2
JIS G3507-1
ASTM A29/A29M
U40152
ML15
ML15
CC15K
C15C
SWRCH15K
1015
TECHNICAL NOTE
Application and ordering note
Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.
RFQ CHECKLIST
What to include in the enquiry
Grade and applicable standard
Diameter or section, delivery condition and quantity
Part drawing, forming stations or failure photos, if available
Testing, certificate or report requirements
RELATED CAPABILITIES
Related manufacturing and quality capabilities
Carbon equivalent calculator — ML15
Basis: GB/T 5953
Chemical composition source: GB/T 6478-2015
Transcribed from the cited standard
Original source wording
Table 1
IIW / CEV
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.1800–0.3467
Missing elements: Mo, V
IIW/CEV: carbon and low-alloy steel weldability screening.
Pcm (Ito–Bessyo)
Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.1483–0.2433
Missing elements: Mo, V, B
Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.
CET
CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.1600–0.2650
Missing elements: Mo
CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.
A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.
Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.
Same-grade reference does not establish standard equivalence, supply or substitution approval.
Standard sources and technical conditions
ML15 · Q/BQB 517-2023
Hot-rolled steel wire rod for cold heading · 6.1.1/Table 1, row 10, note a · PDF page 8 · Mass fraction %
Element
Heat analysis / guide composition
C
0.13~0.18
Si
≤0.1
Mn
0.3~0.6
P
≤0.02
S
≤0.02
Al
≥0.02
Cr
≤0.2
Ni
≤0.2
Cu
≤0.2
Mo
≤0.06
Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 10; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.