Products/ISO 4954

MATERIAL DATA · COLD FORMING

20MoCr4 CHQ wire

Reference technical data for 20MoCr4. Source edition: ISO 4954:2018 · Annex B. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

20MoCr4 CHQ wire product image
20MoCr4 · Cold heading wire
01Applicable standardISO 4954:2018 · Annex B
02Material grade20MoCr4
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

20MoCr4 · ISO 4954:2018

20MoCr4 · ISO 4954:2018 · Mass fraction / %
ElementMass fraction / %
C0.17–0.23
Si≤0.3
Mn0.7–1
P≤0.025
S≤0.025
Cr0.3–0.6
Mo0.4–0.5
Cu≤0.25
Source: ISO 4954:2018
Composition source and applicability · ISO 4954:2018 · PDF 24
ISO 4954:2018 · PDF 24
Composition source and applicability · ISO 4954:2018 · PDF 29
ISO 4954:2018 · PDF 29
Composition source and applicability · ISO 4954:2018 · PDF 30
ISO 4954:2018 · PDF 30
Composition source and applicability · ISO 4954:2018 · PDF 41
ISO 4954:2018 · PDF 41
Composition source and applicability · ISO 4954:2018 · PDF 43
ISO 4954:2018 · PDF 43
Composition source and applicability · ISO 4954:2018 · PDF 44
ISO 4954:2018 · PDF 44
Composition source and applicability · ISO 4954:2018 · PDF 58
ISO 4954:2018 · PDF 58
Composition source and applicability · ISO 4954:2018 · PDF 59
ISO 4954:2018 · PDF 59
Composition source and applicability · ISO 4954:2018 · PDF 60
ISO 4954:2018 · PDF 60

1. Delivery conditions and applicable requirements

Table B.1 – Combinations of heat-treatment condition at delivery, product form and applicable requirements

Delivery conditionSymbolWire rodBarWire
Hot rolled or peeled+AR or +PEXXX
Cold drawn+AR+C—XX
Cold drawn and spheroidize annealed+AR+C+AC—XX
Cold drawn, spheroidize annealed and lightly cold drawn+AR+C+AC+LC—XX
Spheroidize annealed or spheroidize annealed and peeled+AC or +AC+PEXXX
Spheroidize annealed and cold drawn+AC+C—XX
Treated to a ferrite-pearlite structure and specified hardness range+FP—X—

X = applicable; — = not applicable.

Other delivery conditions may be agreed at the time of order.

Applicable requirements according to the basis of order

Ordered with reference to steel names in the tablesRequirement
B.2, B.3, B.4 or B.5Chemical composition according to B.2; mechanical properties according to B.3, B.4 and B.5.
B.2, B.3, B.4, B.5, B.6 or B.7Chemical composition according to B.2; mechanical properties according to B.3, B.4 and B.5; hardenability values according to B.6 and B.7.

Supplementary or special requirements under Annex E apply if agreed at the time of enquiry and order.

Source: ISO 4954:2018, Table B.1, page 22. This table gives the standard relationship between product form, delivery condition and requirements; actual supply must be confirmed separately.

2. Chemical composition

Table B.2 – Chemical composition of case-hardening steels (cast analysis)

These are the standard’s reference requirements for cast analysis of 20MoCr4, not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials of elements that could impair hardenability, mechanical properties or suitability.

Al of 0.020–0.050% may be added to improve cold-heading performance.

a: Single values are maximum limits unless otherwise indicated. A dash does not mean zero content.

b: For steels with hardenability requirements under Tables B.6 and B.7, small departures from the specified limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 2 for the other elements.

c: A lower silicon content or a specified silicon range may be agreed at the time of order.

Source: ISO 4954:2018, Table B.2, page 23 (PDF page 29). The table and notes do not replace the complete standard.

3. Mechanical properties

Table B.5 – Mechanical properties of alloy steels

Steel nameDiameterDelivery condition
+AC+FP+AR+C+AC+AR+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZ min., %HB min.HB max.Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
20MoCr425————5606260060——
20MoCr451056060140187540625806067057
20MoCr4104056060140187540625806066057

Source: ISO 4954:2018, Table B.5, page 27. Rm is tensile strength; Z is reduction of area at fracture. HB denotes Brinell hardness where specified. The values apply only to the specified diameter intervals and delivery conditions.

4. Hardenability requirements

Table B.6 – Hardness limits for steels with normal hardenability (+H)

Steel nameSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.535791113152025303540
20MoCr4+H910max.49474441383533312826252424
20MoCr4+H910min.413731272422———————

Source: ISO 4954:2018, Table B.6, page 29.

Table B.7 – Hardness limits for steels with restricted hardenability bands (+HH and +HL)

Steel nameSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.535791113152025303540
20MoCr4+HH910max.49474441383533312826252424
20MoCr4+HH910min.4440353229262422—————
20MoCr4+HL910max.46444036333129272422212020
20MoCr4+HL910min.413731272422———————

Source: ISO 4954:2018, Table B.7, page 32.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 20MoCr4

Basis: ISO 4954

Chemical composition source: ISO 4954:2018

Transcribed from the cited standard

The technical data and chemical composition on this page cite ISO 4954:2018. Confirm the applicable contract edition separately; do not assume other editions are identical.

Original source wording

Table B.2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.4267–0.6333

Missing elements: V, Ni

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.2467–0.3658

Missing elements: Ni, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.2950–0.4225

Missing elements: Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

Website reference in Chinese (PDF)

20MoCr4 · ISO 683-3:2022

Chemical composition · Cast analysis

Mass fraction %; Table 3, page 18 of the user's PDF. Unlisted elements must not be treated as 0; intentional addition of unlisted elements is subject to the standard and ordering agreement.

ElementMass fraction / %
C0.17~0.23
Si≤0.4
Mn0.7~1
P≤0.025
S≤0.035
Cr0.3~0.6
Mo0.4~0.5
Cu≤0.4

When A.4 is expressly selected in the order, Si≥0.10% may be agreed; the basic table still specifies Si≤0.40%.

Delivery conditions and hardness · Table 7

Brinell hardness. +S: treated to improve shearability; +A: soft annealed; +TH: treated to a specified hardness range; +FP: treated to a ferrite-pearlite structure; +N: normalized. “—” means no requirement is specified for that delivery condition.

Delivery conditionBrinell hardness requirement
+S≤255
+A≤207
+TH156~207
+FP140~187
+N—

Heat treatment and test-piece conditions · Table 8

ItemTemperature / ℃
Austenitizing temperature for the end-quench test910 ± 5
Carburizing temperature (guidance)880~980
Direct and first quenching temperature (guidance)820~860
Second quenching: core quenching temperature (guidance)860~900
Second quenching: case quenching temperature (guidance)780~820
Tempering temperature (guidance)150~200

Except for the end-quench austenitizing temperature, carburizing, quenching and tempering temperatures are guidance values; the actual process must achieve the required properties. Guidance holding times are at least 30 minutes for austenitizing and at least 1 hour for tempering. Select the quenching medium according to product shape, cooling conditions and furnace load.

Hardenability conditions · Tables 5 and 6

Distance from the quenched end in mm; hardness in HRC. Apply only when the corresponding hardenability condition is specified in the order. “—” indicates that no limit is specified at that position.

+H · Normal hardenability
Limit / Distance mm1.535791113152025303540
Maximum49474441383533312826252424
Minimum413731272422———————
+HH · Restricted hardenability band
Limit / Distance mm1.535791113152025303540
Maximum49474441383533312826252424
Minimum4440353229262422—————
+HL · Restricted hardenability band
Limit / Distance mm1.535791113152025303540
Maximum46444036333129272422212020
Minimum413731272422———————
Permissible deviations in product analysis · Table 4
ElementSpecified cast-analysis range / %Permissible product-analysis deviation / %
C0.07<C≤0.31±0.02
Si≤0.40±0.03
Mn≤1.00 / >1.00~1.65±0.04 / ±0.06
P≤0.025+0.005
S≤0.040±0.005
Cr≤1.80±0.05
Mo≤0.30 / >0.30~0.50±0.03 / ±0.04
Ni≤1.00 / >1.00~2.00 / >2.00~3.50±0.03 / ±0.05 / ±0.07
Cu≤0.40+0.05
B≤0.0050±0.0003

“±” permits a deviation for a single cast above the upper limit or below the lower limit, in one direction only. Product-analysis deviations do not change the cast-analysis limits in Table 3.

Standard edition and ordering notes

The standard covers products including wire rod. Finished cold-heading wire supply, processing and properties require technical review and order confirmation. — means not specified in this table, not 0.

Source comparison: reviewed by Codex against the standard supplied by the user. This webpage does not replace the official standard, order agreement or inspection certificate.

WhatsApp Technical enquiry →
Image and content use · Creation Group