1.交货条件的组合
表B.1-交货时热处理条件、产品形式和适用要求的组合
原文表头对照:Heat-treatment condition at delivery=交货热处理状态;Symbol=符号;Wire rod=盘条;Bar=棒材;Wire=钢丝。原标准表格、符号及适用条件保留如下。
Heat-treatment condition at delivery
Symbol
Products form a
Applicable requirements in cases where the steel concerned has been ordered with reference to the steel names indicated in
Wire rod
Bar
Wire
T a b les B. 2,B.3,B.4 or B.5
Ta bles B. 2,B.3,B.4,B.5,B.6 or B,7
Optional
As hot-rolled or peeled
+AR or +PE
X
X
X
Chemical composition as specified in Table B.2
Mechanical properties as specified in Ta b le s B.3 ,B.4 and B.5
Chemical compositior as specified in Table B.2
Mechanical properties as specified in Tables B,3, B.4 and B.5
Values for hardenability according to Ta ble s B.6 and B.7
Supplementa- ry or special requirements as specified in Annex Eh
Cold drawn
+AR+C
-
X
X
Cold drawn + spheroidized
+AR+C+AC
-
X
X
Cold drawn + spheroidized+skin passed
+AR+C+AC +LC
-
X
X
Spheroidized or spheroidized+peeled
+AC or +AC +PE
X
X
X
Spheroidized+cold drawn
+AC+C
X
X
Treated to ferrite- pearlite structure and hardness range
+FP
-
X
-
Others
Other delivery conditions may be agreed at the time of ordering
a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order.
2.化学组成
表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)
表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)
3.力学性能
表B.5-合金钢牌号的力学性能
Steel name
Diameter
Delivery condition
+AC
+FP
+AR+C+AC
+AR+C+AC+LC
+AC+C
above mm
up to mm
Rm max. MPa
Za min %
HB Min.max.
Rm max. MPa
Z min %
Rm max. MPa
Z min. %
Rm max. MPa
Z min. %
20MnCrS5
2
5
— —
—
—
570
62
610
60
—
—
5
10
570
60
152
201
550
62
590
60
680
57
10
40
570
60
152
201
550
62
590
60
670
57
表B.5-合金钢牌号的力学性能 (续)
4.淬透性要求
表B.6-标准淬透性钢种的硬度限值 (H级)
Steel name
Symbol
Austenitizing temperature ℃±5℃
Limits of range
Hardness HRC at a distance from quenched end of test piece(in mm)of
1,5
3
5
7
9
11
13
15
20
25
30
35
40
20MnCrS5
+H
870
max.
49
49
48
46
43
42
41
39
37
35
34
33
32
min.
41
39
36
33
30
28
26
25
23
21
—
—
表B.6-标准淬透性钢种 (H级) 的硬度限值 (续)
表B.7-具有限制淬透性散射带的钢种的硬度限值 (HH和HL等级)
Steel name
Symbol
Austenitizing temperature ℃±5℃
Limits of range
Hardness HRC at a distance from quenched end of test piece(in mm)of