Products/JIS G 3508-2:2005

MATERIAL DATA · COLD FORMING

SWCHB620 Cold heading wire

Technical data for SWCHB620 cold heading wire rod, compliant with JIS G 3508-2:2005. View the chemical composition, mechanical properties, and related technical requirements for this grade.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

SWCHB620 Cold heading wire
SWCHB620 · Cold heading wire
01Applicable standardJIS G 3508-2:2005
02Material gradeSWCHB620
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Chemical Composition

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

Source: JIS G 3508-2:2005 → JIS G 3508-1:2010 · SWRCHB620 · p.4

ElementMass fraction / %
C0.17~0.23
Si0.10~0.35
Mn1.10~1.40
P≤0.030
S≤0.030
B≥0.0008
Cu≤0.30
Ni≤0.20
Cr≤0.20
For all steel grades in this table, Cu shall not exceed 0.30%, Ni 0.20%, and Cr 0.20%. Note a) The lower limit for Si may be set to less than 0.10% by agreement between supplier and purchaser. b) The B content may be 0.0005% or higher by agreement between supplier and purchaser.

2. Hardenability

Table 3 Distance from quenched end and hardness

3. Mechanical properties of wire rod

Table 4 Mechanical properties of wire rod resulting from process D

Notes: 1. For wire diameters exceeding 20 mm, the tolerance is the value in Table 2 minus 5. No tolerance is specified for diameters of 3 mm or less. 2. 1 N/mm² = 1 MPa

Table 5 Mechanical properties of wire rod resulting from the DA process

Notes: 1. For wire diameters exceeding 20 mm, the tolerance is the value in Table 2 minus 5. No tolerance is specified for diameters of 3 mm or less. 2. 1 N/mm² = 1 MPa

4. Decarburized layer depth

Table 6 Permissible limits for average decarburized layer depth

Average decarburized layer depth
Wire diameter (mm)Ferrite decarburized layer depthTotal decarburized layer depth
≤15<0.02<0.15
15<d≤25<0.03<0.20
25<d≤32<0.04<0.25
For SWCH30K to SWCH50K wire, when specified by the purchaser, the test in 10.3.1 shall be performed. The permissible limit for the average decarburized layer depth shall be in accordance with Table 4. However, for wire with a diameter exceeding 32 mm, the limits shall be agreed upon between the supplier and the purchaser.

5. Wire diameter tolerance and out-of-roundness

Table 7 Tolerances and out-of-roundness for wire diameter

Table 7 Wire diameter tolerances and deviations
Unit: mm
Wire diameterPermissible deviationOut-of-roundness
≤30-0.0250.013
3<d≤60-0.0300.013
6<d≤100-0.0360.013
10<d≤180-0.0430.013
18<d≤300-0.0700.013
30<d≤400-0.1000.013
40<d≤500-0.1500.013
Note (3) Out-of-roundness refers to the difference between the maximum and minimum diameters within the same cross-section of the wire.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — SWCHB620

Basis: JIS G 3508-2:2005

Chemical composition source: JIS G 3508-2:2005 → JIS G 3508-1:2010

Transcribed from the cited standard

Original source wording

Table 2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.3533–0.5367

Missing elements: Mo, V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: ≥ 0.2323

Missing elements: Mo, V

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.2800–0.4000

Missing elements: Mo

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →