2 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for SWCHB620 →SWCHB620 · JIS G3508
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Wire rod
- Original record status
- Reference transcription of standard
- Standard edition
- JIS G 3508-2:2005 → JIS G 3508-1:2010
- Table / clause
- Table 2
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.17 ~ 0.23 |
| Si | 0.1 ~ 0.35 |
| Mn | 1.1 ~ 1.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| B | ≥ 0.0008 (upper limit not stated) |
| Cu | ≤ 0.3 (lower limit not stated) |
| Ni | ≤ 0.2 (lower limit not stated) |
| Cr | ≤ 0.2 (lower limit not stated) |
Applicability and limitations
The lower bound for B may be relaxed to 0.0005% by agreement; the lower bound for Si may be below 0.10% by agreement. Composition applies to raw material SWRCHB620. Clause 4 of G3508-2:2005 references G3508-1. The website does not state an edition; the source edition is displayed here without establishing contractual applicability.
Verification notes
Source standard: JIS G 3508-2:2005 → JIS G 3508-1:2010 · Table 2View associated products →SWCHB620 · JIS G 3508-2-2005
Wire naming, citation relationships, and listed historical version compositions have been verified; Confirm separately the contract-applicable editions of undated references
- Material category
- Boron steels
- Material form
- Boron-steel wire for cold heading (SWCHB)
- Verification status
- Original standard verified
- Standard edition
- JIS G 3508-1:2005 (material reference in JIS G 3508-2:2005, Clause 4)
- Table / clause
- Part 1, main-text Table 2 and footnotes; Part 2, main-text Table 1 and note 1—2
- PDF page references
- 3、4、5、6
- Unit
- Mass fraction (wt%)
- Analysis type
- Heat analysis
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Main-text Table 2 of 2005 gives default composition: B≥0.0008%, Si0.10—0.35%
Only when Table 2, note 2 is adopted by agreement: B≥0.0005%; Si remains within the default range, and any low-Si agreement must be checked separately.
Composition record (conditional branches apply; this is not an unconditional requirement)
| Element | Composition requirement |
|---|---|
| C | 0.17 ~ 0.23 |
| Si | 0.1 ~ 0.35 |
| Mn | 1.1 ~ 1.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| B | ≥ 0.0008 (upper limit not stated) |
| Cr | ≤ 0.2 (lower limit not stated) |
| Cu | ≤ 0.3 (lower limit not stated) |
| Ni | ≤ 0.2 (lower limit not stated) |
Applicability and limitations
The original Japanese edition JIS G 3508-2:2005, main-text Table 1 lists SWCHB620 wire; The corresponding wire-rod designation is SWRCHB620, omitting R under Table 1, note 1; these two product forms are not merged. ; Main-text Table 1 permits processes D and DA; D means cold working completed; DA combines cold working and annealing; mechanical values in Table 2/3 must be distinguished by process. ; Clause 4 for this wire references JIS G 3508-1 as the material standard; composition is transcribed from the verified original main-text Table 1/2 in Part 1 of the actual 2005 edition; This is not an independent chemical-composition table in the second part. ; Default B minimum ≥0.0008%; ≥0.0005% applies only by agreement between both parties; Low Si applies only by agreement; agreed limits must not be treated as defaults. ; Mechanical properties in Table 2/3 must be viewed under the separate process and wire-diameter conditions; Decarburization, spheroidization, dimensional and surface requirements are not replaced by this mechanical-table verification; actual supply requires separate confirmation. ; Clause 2 of the second part is an undated reference, pointing to the latest applicable edition; The composition currently shown follows only the obtained and verified historical first-part text from 2005; equivalence with other editions is not established.
Conditional requirement
- Footnote
- Table 5 and Clause 8: dimensions and out-of-roundness
- Source conditions
- Wire diameter d(mm): 0<d≤3, diameter deviation 0/−0.025, out-of-roundness ≤0.013; 3<d≤6,0/−0.030、≤0.015; 6<d≤10,0/−0.036、≤0.018; 10<d≤18,0/−0.043、≤0.022; 18<d≤30,0/−0.070、≤0.035; 30<d≤40,0/−0.100、≤0.050; 40<d≤50,0/−0.150、≤0.070. Out-of-roundness is the difference between the maximum and minimum diameters of the same cross-section; Not ± deviation. >50 is not listed in this table and shall not be extrapolated.
- PDF page references
- 5
- Standard edition
- JIS G 3508-2:2005
- Footnote
- Table 6 and Clause 9: general surface-defect depth
- Source conditions
- 0<d≤50 mm surface defect depth ≤ 0.10 mm; Harmful scale, corrosion, and other defects harmful to use shall still not exist; depth limits shall not be interpreted as permitting all defects. >50 mm not listed in this table.
- PDF page references
- 6
- Standard edition
- JIS G 3508-2:2005
- Footnote
- Table 7: special controls apply only by agreement between both parties
- Source conditions
- Special control subject to agreement between both parties: for 0<d≤15 mm, surface-defect depth ≤0.05 mm.; 15<d≤25 mm≤0.07 mm. >25 mm is not listed in Table 7 and shall not be extrapolated or supplemented with 0; Do not apply the special-control requirements automatically without agreement.. Clauses 10.4 and 10.5 specify the wire diameter and surface inspection methods respectively.
- Subject to agreement
- Yes
- PDF page references
- 6
- Standard edition
- JIS G 3508-2:2005
Original condition-branch records
Main-text Table 2 of 2005 gives default composition: B≥0.0008%, Si0.10—0.35%
| Element | Composition requirement |
|---|---|
| C | 0.17 ~ 0.23 |
| Si | 0.1 ~ 0.35 |
| Mn | 1.1 ~ 1.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| B | ≥ 0.0008 (upper limit not stated) |
| Cr | ≤ 0.2 (lower limit not stated) |
| Cu | ≤ 0.3 (lower limit not stated) |
| Ni | ≤ 0.2 (lower limit not stated) |
Only when Table 2, note 2 is adopted by agreement: B≥0.0005%; Si remains within the default range, and any low-Si agreement must be checked separately.
| Element | Composition requirement |
|---|---|
| C | 0.17 ~ 0.23 |
| Si | 0.1 ~ 0.35 |
| Mn | 1.1 ~ 1.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| B | ≥ 0.0005 (upper limit not stated) |
| Cr | ≤ 0.2 (lower limit not stated) |
| Cu | ≤ 0.3 (lower limit not stated) |
| Ni | ≤ 0.2 (lower limit not stated) |
- Subject to agreement
- Yes
A condition branch must be selected
YesVerification notes
Wire designations in second-part main-text Table 1 and the material reference in Clause 4 have been checked; Composition comes from the original main-text Table 2 in the first part of the same editionMechanical properties applicable to wire process and wire diameter
JIS G 3508-2:2005 · Table 2 Process D, Table 3 Process DA and Notes 1/2; Clause 6 and 10.1/10.2 · PDF pages 4, 6
| Actual process and wire diameter | Upper limit of tensile strength Rm (MPa) | Lower limit of reduction of area Z (%) | Reference hardness HRB (not a guarantee for acceptance) |
|---|---|---|---|
| Process: D; 0<d≤3 mm; HRB≤100 is reference only, not a hardness-acceptance guarantee. The original d≤3 does not specify reduction of area. | ≤ 750 (lower limit not stated) | Not specified in the original source; do not substitute 0 | ≤ 100 (for reference only) |
| Process: D; 3<d<20 mm; HRB≤100 is reference only, not a hardness-acceptance guarantee | ≤ 750 (lower limit not stated) | ≥ 45 (upper limit not stated) | ≤ 100 (for reference only) |
| Process: D; d≥20 mm; HRB≤100 is reference only, not a hardness-acceptance guarantee | ≤ 750 (lower limit not stated) | ≥ 40 (upper limit not stated) | ≤ 100 (for reference only) |
| Process: DA; 0<d≤3 mm; HRB≤94 is reference only, not a hardness-acceptance guarantee. The original d≤3 does not specify reduction of area. | ≤ 630 (lower limit not stated) | Not specified in the original source; do not substitute 0 | ≤ 94 (for reference only) |
| Process: DA; 3<d<20 mm; HRB≤94 is reference only, not a hardness-acceptance guarantee | ≤ 630 (lower limit not stated) | ≥ 55 (upper limit not stated) | ≤ 94 (for reference only) |
| DA process; d≥20 mm. HRB≤94 is for reference only and is not a hardness acceptance guarantee. The reference to Table 2 in footnote DA d≥20 is unresolved; reduction of area is withheld and cannot be assessed automatically against 50% or 40%. | ≤ 630 (lower limit not stated) | Doubts regarding original footnote citations; pending | ≤ 94 (for reference only) |
- Select the actual D/DA process and wire diameter; other processes require agreement between the parties and must not be assumed applicable.
- Rm is an upper tensile-strength limit and Z a lower reduction-of-area limit; Z is not elongation A. 1 N/mm²=1 MPa.
- The entire HRB column is explicitly reference-only in the source; it is not a hardness guarantee.
- For Process D with d≥20 mm, the lower limit of Z is changed from 45 to 40% (reduction of 5); Z is not specified for d≤3 mm; do not fill as 0.
- Note 1 of DA Table 3 refers to Table 2 values. Z at d≥20 mm is withheld pending verification; do not silently change the reference to Table 3 or choose 50/40%.
- Clause 10.1 takes 1 specimen for the same heat, size and heat treatment. Clause 10.2 uses tensile specimen No. 9 under JIS Z2241/Z2201; 9A/9B require agreement. These references are undated; do not invent edition years.
- The decarburization and spheroidization clauses list SWCH30K—SWCH50K, whereas this standard concerns the SWCHB series. Grade applicability remains to be verified; do not automatically apply them to these 12 grades.