SCM440WCH Cold heading wire
SCM440WCH · Cold heading wire
01Applicable standardJIS G 3509-2:2003
02Material gradeSCM440WCH
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Chemical Composition

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

Source: JIS G 3509-2:2003 → JIS G 3509-1:2021 · SCM440RCH · p.7

ElementMass fraction / %
C0.38~0.43
Si0.15~0.35
Mn0.60~0.90
P≤0.030
S≤0.030
Ni≤0.25
Cr0.90~1.20
Mo0.15~0.30
Cu≤0.30
For all steel grades listed in this table, the Cu content as an impurity shall not exceed 0.30%.
Al may be added for grain refinement upon agreement between the supplier and the purchaser.
Elements not specified in this table shall not be intentionally added except for steelmaking purposes; any such addition shall be determined by agreement between the supplier and the purchaser.
Upon agreement between the supplier and the purchaser, the permissible deviations from the specified values for ladle analysis during product analysis of steel shall comply with Table 4 of JIS G 0321.
Note a) The lower limit for Si may be set to a value below 0.15% upon agreement between the supplier and the purchaser.

2. Mechanical properties of wire rod

Table 2 – Mechanical properties of wire rod

GradeTensile strength (N/mm²)Reduction of area (%)
DA1DA2DA3DA1DA2DA3
SCM440WCH≤700-≤640≥55-≥60

3. Depth of decarburized layer

Table 3 Permissible limits for average decarburized layer depth

Unit: mm
DiameterFerrite decarburized layer depthTotal decarburized layer depth
≤15≤0.02≤0.12
>15~25≤0.02≤0.15
>25~32≤0.02≤0.20
>32~40≤0.03≤0.25
>40~50≤0.03≤0.30
For wire rod with a diameter exceeding 50 mm, to be agreed upon by both supplier and purchaser.

4. Hardenability

Table 5 Distance from quenched end and hardness

5. Wire diameter tolerance and out-of-roundness

Table 8 Wire diameter tolerance and out-of-roundness

DiameterPermissible deviationOut-of-roundness
≤15±0.30≤0.40
>15~25±0.40≤0.50
>25~32±0.50≤0.60
>32~50±0.60≤0.70
Note 1) Diameter deviation refers to the difference between the maximum and minimum diameters within the same cross-section of the wire rod. For wire rods with a diameter exceeding 50 mm, this shall be subject to agreement between the supplier and the purchaser.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — SCM440WCH

Basis: JIS G 3509-2:2003

Chemical composition source: JIS G 3509-2:2003 → JIS G 3509-1:2021

Transcribed from the cited standard

Original source wording

Table 2 and its continuation

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.6900–0.9167

Missing elements: V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.4700–0.5858

Missing elements: V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Calculated range: 0.5000–0.6313

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group