Products/ISO 4954

MATERIAL DATA · COLD FORMING

41CrNiMo2 CHQ wire

Reference technical data for 41CrNiMo2. Source edition: ISO 4954:2018 · Annex C. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

Example of a finished or semi-finished part made from Creation Group wire

Original image label: “Finished and semi-finished parts made from Creation Group wire.” The pictured component is illustrative; the image does not verify the material grade of a particular batch.

01Applicable standardISO 4954:2018 · Annex C
02Material grade41CrNiMo2
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Delivery conditions and applicable requirements

Table C.1 – Combinations of heat-treatment condition at delivery, product form and applicable requirements

Delivery conditionSymbolWire rodBarWire
Hot rolled or peeled+AR or +PEXXX
Cold drawn+AR+C—XX
Cold drawn and spheroidize annealed+AR+C+AC—XX
Cold drawn, spheroidize annealed and lightly cold drawn+AR+C+AC+LC—XX
Spheroidize annealed or spheroidize annealed and peeled+AC or +AC+PEXXX
Spheroidize annealed and cold drawn+AC+C—XX
Spheroidize annealed, cold drawn and spheroidize annealed again+AC+C+AC—XX
Spheroidize annealed, cold drawn, spheroidize annealed again and lightly cold drawn+AC+C+AC+LC—XX

X = applicable; — = not applicable.

Other delivery conditions may be agreed at the time of order.

Applicable requirements according to the basis of order

Ordered with reference to steel names in the tablesRequirement
C.2, C.3, C.4, C.5 or C.6Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6.
C.2, C.3, C.4, C.5, C.6, C.7, C.8 or C.9Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; hardenability values according to C.7, C.8 and C.9.
C.2, C.3, C.4, C.5, C.6 or C.10Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; minimum core hardness and maximum diameter according to C.10.

Supplementary or special requirements under Annex E apply if agreed at the time of enquiry and order.

Source: ISO 4954:2018, Table C.1, page 34. This table gives the standard relationship between product form, delivery condition and requirements; actual supply must be confirmed separately.

2. Chemical composition

Table C.2 – Chemical composition of steels without boron for quenching and tempering (cast analysis)

These are the standard’s reference requirements for cast analysis of 41CrNiMo2, not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

ElementMass fraction, %
C0.37–0.44
Si≤0.30
Mn0.70–1.00
P≤0.025
S≤0.025
Cr0.40–0.60
Ni0.40–0.70
Mo0.15–0.30
Cu≤0.25

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials of elements that could impair hardenability, mechanical properties or suitability.

Al of 0.020–0.050% may be added to improve cold-heading performance.

a: Single values are maximum limits unless otherwise indicated. A dash does not mean zero content.

b: For steels with hardenability requirements under Tables C.7 and C.9, small departures from the specified limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 2 for the other elements.

c: A carbon range 0.04 percentage points wide, for example 0.33–0.37%, may be agreed at the time of enquiry and order.

d: A lower silicon content may be agreed at the time of order. Its effects on the specified properties, such as hardenability, must then be assessed.

Source: ISO 4954:2018, Table C.2, page 35 (PDF page 41). The table and notes do not replace the complete standard.

3. Mechanical properties

Table C.5 – Mechanical properties of alloy steels without boron

Steel nameDiameterDelivery condition
+AC or +AC+PE+AC+C+AC+AC+C+AC+LC
over, mmup to and including, mmRm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
41CrNiMo225——6406068055
41CrNiMo2540——6406068055

Source: ISO 4954:2018, Table C.5, page 40. Rm is tensile strength; Z is reduction of area at fracture. The values apply only to the specified diameter intervals and delivery conditions.

4. Hardenability requirements

Table C.7 – Hardness limits for steels without boron with specified normal hardenability (+H)

Steel nameSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
12345678910111315202530
41CrNiMo2+H850max.606060595857555448424038373736—
41CrNiMo2+H850min.535352504742383530282625242423—

Source: ISO 4954:2018, Table C.7, page 45.

Table C.9 – Hardness limits for steels without boron with restricted hardenability bands (+HH and +HL)

Steel nameSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
41CrNiMo2+HH850max.606060595857555448424038373736
41CrNiMo2+HH850min.555555535147444136333129282827
41CrNiMo2+HL850max.585857565452494842373534333332
41CrNiMo2+HL850min.535352504742383530282625242423

a: This table does not apply to steels ordered with a restricted carbon range; see footnote c to Table C.2.

Source: ISO 4954:2018, Table C.9, page 49.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 41CrNiMo2

Basis: ISO 4954

Chemical composition source: ISO 4954:2018

Transcribed from the cited standard

Original source wording

Table C.2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.6233–0.8500

Missing elements: V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.4417–0.5742

Missing elements: V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Calculated range: 0.4850–0.6300

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group