Technical data for SNC631WCH Cold heading wire, compliant with JIS G 3509-2:2003. View chemical composition, mechanical properties, and related technical requirements for this grade.
Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.
Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.
Source: JIS G 3509-2:2003 → JIS G 3509-1:2021 · SNC631RCH · p.7
Element
Mass fraction / %
C
0.27~0.35
Si
0.15~0.35
Mn
0.35~0.65
P
≤0.030
S
≤0.030
Ni
2.50~3.00
Cr
0.60~1.00
Cu
≤0.30
For all steel grades listed in this table, the Cu content as an impurity shall not exceed 0.30%. Al may be added for grain refinement upon agreement between the supplier and the purchaser. Elements not specified in this table shall not be intentionally added except for steelmaking purposes; any such addition shall be determined by agreement between the supplier and the purchaser. Upon agreement between the supplier and the purchaser, the permissible deviations from the specified values for ladle analysis during product analysis of steel shall comply with Table 4 of JIS G 0321. Note a) The lower limit for Si may be set to a value below 0.15% upon agreement between the supplier and the purchaser.
2. Mechanical properties of wire rod
Table 2 – Mechanical properties of wire rod
Grade
Tensile strength (N/mm²)
Reduction of area (%)
DA1
DA2
DA3
DA1
DA2
DA3
SNC631WCH
≤650
-
≤620
≥60
-
≥60
3. Depth of decarburized layer
Table 3 Permissible limits for average decarburized layer depth
Unit: mm
Diameter
Ferrite decarburized layer depth
Total decarburized layer depth
≤15
≤0.02
≤0.12
>15~25
≤0.02
≤0.15
>25~32
≤0.02
≤0.20
>32~40
≤0.03
≤0.25
>40~50
≤0.03
≤0.30
For wire rod with a diameter exceeding 50 mm, to be agreed upon by both supplier and purchaser.
4. Hardenability
Table 5 Distance from quenched end and hardness
5. Wire diameter tolerance and out-of-roundness
Table 8 Wire diameter tolerance and out-of-roundness
Diameter
Permissible deviation
Out-of-roundness
≤15
±0.30
≤0.40
>15~25
±0.40
≤0.50
>25~32
±0.50
≤0.60
>32~50
±0.60
≤0.70
Note 1) Diameter deviation refers to the difference between the maximum and minimum diameters within the same cross-section of the wire rod. For wire rods with a diameter exceeding 50 mm, this shall be subject to agreement between the supplier and the purchaser.
TECHNICAL NOTE
Application and ordering note
Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.
RFQ CHECKLIST
What to include in the enquiry
Grade and applicable standard
Diameter or section, delivery condition and quantity
Part drawing, forming stations or failure photos, if available
Testing, certificate or report requirements
RELATED CAPABILITIES
Related manufacturing and quality capabilities
Carbon equivalent calculator — SNC631WCH
Basis: JIS G 3509-2:2003
Chemical composition source: JIS G 3509-2:2003 → JIS G 3509-1:2021
Transcribed from the cited standard
Original source wording
Table 2 and its continuation
IIW / CEV
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.6150–0.8783
Missing elements: Mo, V
IIW/CEV: carbon and low-alloy steel weldability screening.
Pcm (Ito–Bessyo)
Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.3642–0.5092
Missing elements: Mo, V, B
Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.
CET
CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.3975–0.5550
Missing elements: Mo
CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.
A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.
Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.