Products/GB/T 5953

MATERIAL DATA · COLD FORMING

ML35 Cold heading wire

Reference technical data for ML35. Source edition: GB/T 5953.1-2009. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

Example of a finished or semi-finished part made from Creation Group wire

Original image label: “Finished and semi-finished parts made from Creation Group wire.” The pictured component is illustrative; the image does not verify the material grade of a particular batch.

01Applicable standardGB/T 5953.1-2009
02Material gradeML35
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Chemical Composition

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

Source: GB/T 6478-2015 · ML35 · p.9

ElementMass fraction / %
C0.33~0.38
Si0.10~0.30
Mn0.60~0.90
P≤0.025
S≤0.025

2. Mechanical Properties

Table 3 – Mechanical properties of carbon steel wire intended for quenching and tempering

Reference edition: GB/T 5953.1-2009, Table 3. Under clause 3.2, SALD means cold drawn, spheroidize annealed and lightly drawn; SA means cold drawn and spheroidize annealed. These reference data do not establish compliance with a different edition or the condition of a delivered heat.

Grade a)Diameter/mmSALDSA
Tensile strength Rm/MPaReduction of area Z / %Rockwell hardness/HRBTensile strength Rm MPaReduction of area Z / %Rockwell hardness/HRB
ML25 ML25Mn ML30Mn ML30 ML35≤6.00490-690≥55-380-560≥60≤86
>6.00-12.00470-650≥55-
>12.00-25.00450-600≥50≤89
a) The chemical composition of the grade may refer to GB/T 6478.

2.1 For wire delivered in the HD condition, mechanical properties shall be determined by agreement between the supplier and the purchaser.
2.2 The mechanical properties of quenched and tempered steel wire in the delivery condition shall comply with the provisions of Table 3 and Table 4.
2.3 When wire is delivered in straight lengths or in a polished condition, a 10% variation in mechanical properties is permitted.
2.4 For wire with a nominal diameter greater than 25.00 mm, the mechanical properties shall be determined by agreement between the supplier and the purchaser.
2.5 The mechanical properties for grades not listed in the table shall be determined by agreement between the supplier and the purchaser.
2.6 Upsetting: Wire samples shall be cold upset to one-half of their original height without surface cracks or fissures. By mutual agreement, upsetting may also be performed to one-third or one-quarter of the original sample height.

3. Microstructure

Table 6 Permissible range for decarburized layer depth

For spheroidizing annealed wire, the spheroidized microstructure may be inspected upon the purchaser's request and as specified in the contract; the acceptance criteria and test methods shall be agreed upon by the supplier and the purchaser.

Nominal diameter of wireDepth of complete decarburizationTotal decarburized layer depth
≤8.00≤0.02≤0.10
>8.00-15.0≤0.02≤0.15
>15.0-25.0≤0.03≤0.20
>25.0-45.0By agreementBy agreement

3.1 Decarburized layer: Upon the purchaser's request and as specified in the contract, the decarburized layer on the wire surface may be inspected. The permissible depth of the total decarburized layer (ferrite + transition zone) and the complete decarburized layer on one side shall comply with Table 6. Special requirements for the decarburized layer shall be determined by agreement between the supplier and the purchaser. For wire grades with a carbon content not greater than 0.30%, the test method shall be agreed upon by the supplier and the purchaser.
3.2 Carburization: The wire surface shall be free from carburization. Inspection may be omitted if the supplier can provide assurance.

4. Surface quality


4.1 The wire surface shall be smooth and free from cracks, scabs, folds, laminations, drawing marks, and rust. However, individual pits, raised surfaces, indentations, and scratches with a depth not exceeding half the diameter tolerance are permitted. Wire delivered in the annealed condition may exhibit oxidation colors on the surface.
4.2 Requirements for wire surface coatings shall be determined by mutual agreement between the supplier and the purchaser.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — ML35

Basis: GB/T 5953

Chemical composition source: Original standard not yet verified

Original standard not yet verified

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

Standard sources and technical conditions

ML35 · Q/BQB 517-2023

Hot-rolled steel wire rod for cold heading · 6.1.1/Table 1, row 43, note a · PDF page 10 · Mass fraction %

ElementHeat analysis / guide composition
C0.32~0.39
Si≤0.2
Mn0.3~0.6
P≤0.02
S≤0.02
Cr≤0.2
Ni≤0.2
Cu≤0.2
Mo≤0.06

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 43; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Original source: Q/BQB 517—2023