Products/ASTM F2282

MATERIAL DATA · COLD FORMING

IFI-1022/B Cold-Heading Steel Wire

Reference technical data for IFI-1022/B. Source edition: ASTM F2282-18. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

Example of a finished or semi-finished part made from Creation Group wire

Original image label: “Finished and semi-finished parts made from Creation Group wire.” The pictured component is illustrative; the image does not verify the material grade of a particular batch.

01Applicable standardASTM F2282-18
02Material gradeIFI-1022/B
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Chemical composition and applicable practices

IFI-1022/B reference requirements under ASTM F2282-18; mass fraction in percent. These are not measured heat-analysis results. Legacy SAE/AISI catalogue labels do not establish equivalence: ASTM F2282 explicitly notes that IFI composition ranges may differ from SAE or AISI ranges. Confirm the exact grade, edition and requirements in the order.

Table 4 – Chemical ranges and limits

IFI gradeC min.C max.Mn min.Mn max.P max.S max.
IFI-1022/B0.200.230.901.100.0200.020

A dash means no numerical limit is specified in this source cell; it does not mean zero content.

Permitted conditions furnished: AlK, SiFg, SiCg. AlK = aluminum killed; R = rimmed steel; SiFg = silicon-killed fine-grain practice; SiCg = silicon-killed coarse-grain practice; CgP = coarse-grain practice.

Table 6 – Silicon limits for this grade’s permitted practices, %

Deoxidation/grain practiceSilicon limit
AlK≤0.10
SiFg0.15–0.30
SiCg0.15–0.30

The /B suffix identifies a grade group; it is not the boron designator between digits. For steels without intentional boron or titanium additions, Table 9 gives B ≤0.0007% and Ti ≤0.01%.

Table 5 – Permissible variations for product analysis, %

ElementSpecified limit/rangePermissible variation
C≤0.25±0.02
C>0.25 and ≤0.55±0.03
Mn≤0.90±0.03
Mn>0.90 and ≤1.65±0.06
PAbove maximum only+0.008
SAbove maximum only+0.008
Si≤0.30±0.02
CuAbove maximum only+0.03
SnAbove maximum only+0.01
NiAbove maximum only+0.03
CrAbove maximum only+0.03
MoAbove maximum only+0.01
VAbove maximum only+0.01
BNot applicable unless misapplication is indicatedN/A

For a range, the variation may occur above the maximum or below the minimum; results for the same heat must not vary in both directions. For phosphorus and sulfur, only an excess above the specified maximum is permitted within the listed allowance. Under clause 6.4.2, product analysis is generally unsuitable for carbon, phosphorus and sulfur in rimmed or capped steels unless misapplication is clearly indicated. Source: ASTM F2282-18, clause 6 and Tables 4–9, pages 3–5.

2. Mechanical properties

Table 11 – IFI-1022/B in the specified delivery conditions

Material conditionMaximum tensile strength, ksiMinimum reduction of area, %
Wire rod/bar – annealed7362
Wire rod/bar – spheroidize annealed6965
Wire – spheroidize annealed at finished size (SAFS)6768
Wire – annealed in process, then lightly drawn to finished size (AIP)8260
Wire – spheroidize annealed in process, then lightly drawn to finished size (SAIP)7362

For aluminum-killed steel, subtract 3 ksi from the tensile-strength limit and add 1 percentage point to the reduction-of-area minimum. For rimmed steel, subtract 5 ksi and add 2 percentage points, respectively. For AIP and SAIP wire below 0.200 in., add 50 psi to the tensile-strength limit for every 0.001 in. below 0.200 in. Reduction-of-area testing does not apply to wire below 0.092 in. Source: ASTM F2282-18, Table 11, page 9. The table uses ksi, while the diameter adjustment uses psi; these units are not interchangeable.

3. Microstructure and spheroidization

Clause 7.3.1 requires a minimum spheroidization rating of G2 or L2 against IFI Plate 1. Clause 7.3.2 describes spheroidization of at least 90% as optimum; it is not a separate mandatory 90% acceptance threshold. Percentage ratings are approximate visual assessments. Austenitic grain size and testing must follow the specified practice and ASTM E112. Source: ASTM F2282-18, clauses 7.2–7.3 and Plate 1, pages 4–7.

4. Decarburization limits

Table 10 applies to killed steels with carbon content exceeding 0.15%. Applicability must be assessed for the actual grade, heat composition and condition. All diameters and depths in this table are in inches; they are not millimetres.

Nominal diameter, in.Maximum free-ferrite depth, in.Maximum total average affected depth (TAAD), in.Maximum worst-location depth, in.
≤25/640.0010.0050.008
>25/64 and ≤5/80.0010.0060.009
>5/8 and ≤55/640.0010.0070.011
>55/64 and ≤10.0010.0080.012
>1 and ≤1½0.0010.0100.015

Measure and evaluate decarburization according to Section 8. Source: ASTM F2282-18, Table 10, page 8. TAAD and worst-location depth are separate limits; neither is a case-hardening depth.

5. Surface condition and coating

Mill scale on hot-rolled material must be removable by acid pickling or mechanical descaling. Surface contaminants must not impede cleaning or contaminate the pickle bath. Bar, rod and wire must be free from detrimental imperfections such as seams, voids, pits, scratches and laps. Coating requirements are specified by the purchaser for the forming process and order. Source: ASTM F2282-18, Sections 11–13, page 8.

These excerpts are standard references, not batch certificates, a supply commitment or approval of material substitution. The complete standard and technical order agreement govern the assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — IFI-1022/B

Basis: ASTM F2282

Chemical composition source: ASTM F2282-18

Transcribed from the cited standard

Original source wording

Table 4 / Table 6 / Table 9

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.3500–0.4613

Missing elements: V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.2490–0.3193

Missing elements: Si, V

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Calculated range: 0.2900–0.3615

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →