Products/EN 10263

MATERIAL DATA · COLD FORMING

42CrMoS4 Cold-drawn steel wire

Reference technical data for 42CrMoS4. Source edition: EN 10263-4:2017. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

42CrMoS4 Cold-drawn steel wire product image
42CrMoS4 · Cold-drawn steel wire
01Applicable standardEN 10263-4:2017
02Material grade42CrMoS4
03Product formCold-drawn steel wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

42CrMoS4 · EN 10263-4-2017

42CrMoS4 · EN 10263-4-2017 · Mass fraction / %
ElementMass fraction / %
C0.38–0.45
Si≤0.3
Mn0.6–0.9
P≤0.025
S0.02–0.04
Cu≤0.25
Cr0.9–1.2
Mo0.15–0.3

42CrMoS 4 · DIN EN 10263-4-2002

42CrMoS 4 · DIN EN 10263-4-2002 · Mass fraction / %
ElementMass fraction / %
C0.38–0.45
Si≤0.3
Mn0.6–0.9
P≤0.025
S0.02–0.04
Cu≤0.25
Cr0.9–1.2
Mo0.15–0.3

42CrMoS4 · EN 10263-4-2001

42CrMoS4 · EN 10263-4-2001 · Mass fraction / %
ElementMass fraction / %
C0.38–0.45
Si≤0.3
Mn0.6–0.9
P≤0.025
S0.02–0.04
Cu≤0.25
Cr0.9–1.2
Mo0.15–0.3
Source: EN 10263-4-2017
Composition source and applicability · EN 10263-4-2017 · PDF 9
EN 10263-4-2017 · PDF 9
Composition source and applicability · EN 10263-4-2017 · PDF 10
EN 10263-4-2017 · PDF 10
Source: DIN EN 10263-4-2002 / EN 10263-4-2001
Composition source and applicability · DIN EN 10263-4-2002 / EN 10263-4-2001 · PDF 8
DIN EN 10263-4-2002 / EN 10263-4-2001 · PDF 8

1. Delivery conditions and applicable requirements

Table 1 – Delivery conditions, product forms and applicable requirements

Heat-treatment conditionSymbolBarWire rodWire
UntreatedNone or +UXX—
Spheroidize annealed+ACXXX
Basis of orderApplicable requirements
Table 3 and 4, 6 or 7 or 8Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8.
Table 3 and 4, 6 or 7 or 8, 9 or 10 or 11Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8; hardenability according to Table 9, 10 or 11.
Table 3 and 4, 6 or 7 or 8, 12Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8; minimum core hardness and maximum diameter according to Table 12.
Table 3, 4, 6, 7, 8, 9, 10, 11 or 12Supplementary or special requirements under Annex A of EN 10263-1, if agreed at the time of enquiry and order.

Table 2 – Surface condition at delivery

Basis of agreementSurface conditionSymbolBarWire rodWire
Unless otherwise agreedAs rolledNone or +ARXX—
Special surface condition by agreementCold drawn+C——X
Special surface condition by agreementLightly cold drawn+LCX—X
Special surface condition by agreementPeeled+PEXXX

X = applicable; — = not applicable. Other delivery conditions may be agreed at the time of order.

Heat-treatment condition and surface condition are separate requirements. This table gives the standard reference; the actual product form, delivery condition and suitability must be confirmed in the order.

Source: EN 10263-4:2017, Table 1 and 2, page 6–7 (PDF page 7–8).

2. Chemical composition

Table 3 – Chemical composition of steels without boron (cast analysis)

Reference requirements for 42CrMoS4, steel number 1.7227. These are not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

Values are mass fractions in percent. Single values are maximum limits unless otherwise indicated. “—” represents a blank source field and does not mean zero content.

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials that could impair hardenability, mechanical properties or suitability.

For steels with hardenability requirements under Tables 9–11, small departures from the composition limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 5 for the other elements.

An aluminium addition of 0.020–0.050% is possible to improve cold-heading performance.

A lower silicon content may be agreed at the time of order. Its effect on the specified properties, such as hardenability, must be assessed.

A carbon range 0.04 percentage points wide, for example 0.33–0.37%, may be agreed at the time of enquiry and order.

Table 5 – Permissible deviations for product analysis

ElementLimiting values for cast analysis, %Permissible deviation for product analysis, %
C≤0.50±0.02
Si≤0.30±0.03
Mn≤1.00±0.04
Mn>1.00 and ≤1.45±0.05
P≤0.025+0.005
S≤0.025+0.005
Cr≤1.70±0.05
Mo≤0.30±0.03
Ni≤2.00±0.05
B≤0.0050±0.0003
Cu≤0.25+0.03

± means that, within one heat, the product analysis for an element may deviate above the upper limit or below the lower limit in Tables 3 and 4, but not in both directions at the same time.

For steels with a specified sulfur range of 0.020–0.035% or 0.020–0.040% in the cast analysis, the permissible deviation is ±0.005%.

Source: EN 10263-4:2017, Table 3 on page 8 (PDF page 9), and Table 5 on page 10 (PDF page 11). These tables do not replace the complete standard.

Dimensions and shape / Mechanical properties

Confirm size, tolerance class, delivery condition and inspection conditions in the drawing or technical agreement.

Dimensional bands

EN 10263-1:2017 §8 → EN 10218-2:2012 §§4.1.1–4.1.2 · Table 1

For bright drawn round wire, excluding organically coated wire. T3, T4 and T5 are reference alternatives selected on order; agree other classes, surface conditions and d >25 mm.

Δ = ±t; dmax − dmin ≤ t; 0.05 ≤ d ≤ 25 mm

Dimensional bands · T3 / T4 / T5
T3 · mm
Diameter rangeDiameter toleranceMaximum out of round
0.05 ≤ d < 0.12± 0.006≤ 0.006
0.12 ≤ d < 0.15± 0.008≤ 0.008
0.15 ≤ d < 0.23± 0.01≤ 0.01
0.23 ≤ d < 0.33± 0.012≤ 0.012
0.33 ≤ d < 0.52± 0.015≤ 0.015
0.52 ≤ d < 0.91± 0.02≤ 0.02
0.91 ≤ d < 1.42± 0.025≤ 0.025
1.42 ≤ d < 2.05± 0.03≤ 0.03
2.05 ≤ d < 2.78± 0.035≤ 0.035
2.78 ≤ d < 3.63± 0.04≤ 0.04
3.63 ≤ d < 4.6± 0.045≤ 0.045
4.6 ≤ d < 5.67± 0.05≤ 0.05
5.67 ≤ d < 8.17± 0.06≤ 0.06
8.17 ≤ d < 11.12± 0.07≤ 0.07
11.12 ≤ d < 14.52± 0.08≤ 0.08
14.52 ≤ d < 18.37± 0.09≤ 0.09
18.37 ≤ d < 22.68± 0.1≤ 0.1
22.68 ≤ d ≤ 25± 0.12≤ 0.12
T4 · mm
Diameter rangeDiameter toleranceMaximum out of round
0.05 ≤ d < 0.072± 0.004≤ 0.004
0.072 ≤ d < 0.12± 0.005≤ 0.005
0.12 ≤ d < 0.17± 0.006≤ 0.006
0.17 ≤ d < 0.29± 0.008≤ 0.008
0.29 ≤ d < 0.45± 0.01≤ 0.01
0.45 ≤ d < 0.65± 0.012≤ 0.012
0.65 ≤ d < 1.01± 0.015≤ 0.015
1.01 ≤ d < 1.78± 0.02≤ 0.02
1.78 ≤ d < 2.78± 0.025≤ 0.025
2.78 ≤ d < 4.01± 0.03≤ 0.03
4.01 ≤ d < 5.45± 0.035≤ 0.035
5.45 ≤ d < 7.12± 0.04≤ 0.04
7.12 ≤ d < 9.01± 0.045≤ 0.045
9.01 ≤ d < 11.12± 0.05≤ 0.05
11.12 ≤ d < 16.01± 0.06≤ 0.06
16.01 ≤ d < 21.77± 0.07≤ 0.07
21.77 ≤ d ≤ 25± 0.08≤ 0.08
T5 · mm
Diameter rangeDiameter toleranceMaximum out of round
0.05 ≤ d < 0.091± 0.003≤ 0.003
0.091 ≤ d < 0.17± 0.004≤ 0.004
0.17 ≤ d < 0.26± 0.005≤ 0.005
0.26 ≤ d < 0.37± 0.006≤ 0.006
0.37 ≤ d < 0.65± 0.008≤ 0.008
0.65 ≤ d < 1.01± 0.01≤ 0.01
1.01 ≤ d < 1.45± 0.012≤ 0.012
1.45 ≤ d < 2.26± 0.015≤ 0.015
2.26 ≤ d < 4.01± 0.02≤ 0.02
4.01 ≤ d < 6.26± 0.025≤ 0.025
6.26 ≤ d < 9.01± 0.03≤ 0.03
9.01 ≤ d < 12.26± 0.035≤ 0.035
12.26 ≤ d < 16.01± 0.04≤ 0.04
16.01 ≤ d < 20.26± 0.045≤ 0.045
20.26 ≤ d ≤ 25± 0.05≤ 0.05

Mechanical-property bands

EN 10263-4:2017 · Table 7 · PDF 12

+AC: spheroidizing annealed · +C: cold drawn · +LC: lightly drawn

Mechanical-property bands · 42CrMoS4
Delivery condition / processDiameter range (mm)Tensile strength Rm (MPa)Reduction of area Z (%)
+AC2 < d ≤ 5——
+AC5 < d ≤ 40≤ 630≥ 58
+AC+C+AC2 < d ≤ 5≤ 620≥ 60
+AC+C+AC5 < d ≤ 40≤ 610≥ 60
+AC+C+AC+LC2 < d ≤ 5≤ 660≥ 58
+AC+C+AC+LC5 < d ≤ 40≤ 650≥ 58

—: Not specified in this table. Do not extrapolate across delivery states or sizes; these are not measured batch results.

4. Hardenability requirements

Table 9 – Hardness limits for steels without boron with normal hardenability (+H)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
42CrMoS41.7227+H850max.616161606059595856535148474645
42CrMoS41.7227+H850min.535352514943403734323130302929

Source: EN 10263-4:2017, Table 9, page 16.

Table 10 – Hardness limits for steels without boron with restricted hardenability bands (+HH and +HL)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
42CrMoS41.7227+HH850max.616161606059595856535148474645
42CrMoS41.7227+HH850min.565655545248464441393836363534
42CrMoS41.7227+HL850max.585858575654535149464442414040
42CrMoS41.7227+HL850min.535352514943403734323130302929

Table 10 does not apply to steels ordered with a restricted carbon range under note b to Table 3.

Source: EN 10263-4:2017, Table 10, page 18.

Table 12 – Maximum diameter for at least 90% martensite in the core-hardening test (+CH)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C), see note aMinimum core hardness, HRCMaximum diameter, mm, see note b
42CrMoS41.7227+CH8505021

As a guide, a holding time of at least 30 minutes at the specified hardening temperature is recommended.

The maximum diameters apply to the lowest hardenability within each steel grade. For +HH qualities, the maximum diameter may be increased.

Source: EN 10263-4:2017, Table 12, page 21.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 42CrMoS4

Basis: EN 10263

Chemical composition source: EN 10263-4:2017 · Table 3

Transcribed from the cited standard

Composition is taken from the reviewed Table 3 above. The row for 42CrMoS4, steel number 1.7227, was checked against BS EN 10263-4:2017, PDF page 9 (printed page 8). Unknown elements remain unknown. Confirm the applicable contract edition separately.

Source table reference

EN 10263-4:2017, Table 3

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.6900–0.9167

Missing elements: V, Ni

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.4650–0.5975

Missing elements: Ni, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.5000–0.6425

Missing elements: Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group