42CRMOS4
16 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for 42CRMOS4 →42CrMoS4 · DIN 17200-1987
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Alloy steel
- Subcategory
- Alloy steel
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- DIN 17200-1987-03
- Table / clause
- Table 2 and footnotes 1–5; 7.3.1–7.3.2
- PDF page references
- 1、2、15、16、17
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Mn | 0.6 ~ 0.9 |
| S | 0.02 ~ 0.035 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Si | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.035 (lower limit not stated) |
Applicability and limitations
Table 2 cast analysis, mass fraction wt%; Si is an upper limit and unspecified elements are not filled with zero. P/S requirements for the C, Ck and Cm series remain separate; S 0.020–0.035% in S-containing grades is a two-sided range. Note 1: unlisted elements may not be intentionally added without purchaser consent, except to complete melting; no fixed residual values are inferred. Table 3 contains permissible product-analysis deviations, not added to cast limits; applicable sizes and positive/negative directions are checked separately. Heat-treatment condition, hardenability and size-dependent properties require separate verification. The standard includes hot-rolled wire rod; chemistry alone is no cold-heading supply commitment. Note 2: small composition deviations, excluding P/S, may be agreed when ordering restricted hardenability bands or quenched-and-tempered/normalized properties, but may not exceed Table 3. These data retain the Table 2 baseline without automatic relaxation. Light-typeface grades in note 4 are for special applications only. Note 5 permits separate ordering of Pb 0.15–0.30% only for the marked C-series grades; not added to ordinary base compositions. Original material number 1.7227; not marked for special application under note 4.
Verification notes
March 1987, Table 2 and all footnotes transcribed; mechanical properties checked separately.42CrMoS4 · ISO 4954
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Cold-heading wire
- Original record status
- Source edition identified; composition verification pending
- Standard edition
- ISO 4954:2018
- Table / clause
- Table C.2
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Cu | ≤ 0.25 (lower limit not stated) |
Applicability and limitations
Composition based on ISO 4954:2018; the product edition is unspecified, so confirm the edition applicable to the contract.
Composition conditions
- ISO 4954:2018, Table C.2 gives heat analysis; A single value is a maximum; a dash is not zero.
- Product-analysis tolerances are listed separately under Table 2/3 of the standard and do not directly widen the heat-analysis composition ranges.
- Optional Al0.020–0.050% to improve cold-heading performance; this is not a universal mandatory minimum.
- Low Si may be agreed in the order, taking hardenability into account; Where hardenability is required, the standard permits limited deviations, except for P/S; C must not exceed 0.01%; see Table 2 for the other requirements.
- For C, a range of width 0.04% may be agreed; it does not replace the tabulated range by default.
Verification notes
Composition based on ISO 4954:2018; the product edition is unspecified, so confirm the edition applicable to the contract.View associated products →42CrMoS4 · ISO 4954-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Alloy steel
- Subcategory
- Steel for quenching and tempering
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 4954:2018
- Table / clause
- Table C.2
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Cu | ≤ 0.25 (lower limit not stated) |
Applicability and limitations
ISO 4954:2018, Table C.2 gives heat analysis; A single value is a maximum; a dash is not zero. ; Product-analysis tolerances are listed separately under Table 2/3 of the standard and do not directly widen the heat-analysis composition ranges. ; Optional Al0.020–0.050% to improve cold-heading performance; this is not a universal mandatory minimum. ; Low Si may be agreed in the order, taking hardenability into account; Where hardenability is required, the standard permits limited deviations, except for P/S; C must not exceed 0.01%; see Table 2 for the other requirements. ; For C, a range of width 0.04% may be agreed; it does not replace the tabulated range by default.
Verification notes
Table C.2 and its footnotes in the standard text were checked.42CrMoS4 · ISO 4954-1-2024
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 4954-1-2024
- Table / clause
- Table C.2 and notes a–d
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Default heat composition in Table C.2/C.3
Uses an addition of Al intended to improve cold-heading performance, Al≤0.050%
Composition record (conditional branches apply; this is not an unconditional requirement)
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
Mass fraction wt%; Table C.2/C.3 heat analysis; see Table 2 separately for product-analysis tolerances. ; Note a: Al≤0.050% may be added to improve cold heading, but is not mandatory by default. ; Note c: A lower Si or a specified Si range may be requested by agreement; specific agreements have not yet been provided and shall not be filled in arbitrarily. ; When hardenability requirements exist, the small deviations permitted in Table B.6/B.7 must be verified separately according to Table 2 and conditions; the default composition range shall not be expanded. ; Elements not listed must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; Unspecified values are not treated as zero. ; Mechanical properties/hardenability have not been supplemented in this batch; Cold heading applicability must be determined in conjunction with dimensions, state, and technical conditions.
Original condition-branch records
Default heat composition in Table C.2/C.3
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Uses an addition of Al intended to improve cold-heading performance, Al≤0.050%
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Al | ≤ 0.05 (lower limit not stated) |
A condition branch must be selected
YesVerification notes
The original English text of 2024, Table C.2/C.3 and footnotes have been checked42CrMoS4 · EN 10263-4-2017
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- EN 10263-4-2017
- Table / clause
- Table 3 and notes
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Default heat composition listed in the table; optional Al addition not selected.
Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.
Composition record (conditional branches apply; this is not an unconditional requirement)
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
EN10263-4:2017, Table 3, heat analysis, mass percent. ; Elements not listed shall not be filled as 0; they shall not be intentionally added without the consent of the purchaser, except additions needed to finish steelmaking. ; Note 2 allows the specification of small deviations when hardenability requirements exist, but this does not involve P/S; The default composition range is not expanded here; it must be combined with specific hardenability ordering conditions. ; Note 3 allows Al 0.020–0.050% to be listed separately; it shall not be defaulted as mandatory aluminum content. ; Mechanical properties and delivery conditions are to be verified separately; the standard range is not a guarantee for the forming of arbitrary parts. ; Note a: lower Si may be agreed upon, but the influence on properties such as hardenability must be considered; do not fill in if no specific agreement range is provided. ; Note b allows a C range of 0.04% width by agreement; the example .33–.37 is not a uniform range for all grades.
Original condition-branch records
Default heat composition listed in the table; optional Al addition not selected.
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Al | 0.02 ~ 0.05 |
A condition branch must be selected
YesVerification notes
Visual check of Tables 3 and 4 and footnotes in the English original42CrMoS4 · DIN EN 10263-4-2002
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- DIN EN 10263-4-2002
- Table / clause
- Table 2
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
DIN EN10263-4:2002-02 adopts EN10263-4:2001; the edition relationship is expressly identified on the cover; Heat-analysis mass percentages. ; Historical Table 2/3 contains no optional Al addition note for 2017; newer-edition conditions are not applied. ; Table 2, note c permits an agreed carbon range of width .04%; tabulated defaults are unchanged without a specific agreement. ; Table 2, note d and Table 3, note c permit agreed lower Si, considering effects on properties/hardenability; no range is invented where none is specified. ; Unlisted elements are not entered as zero; Table 2, note a: intentional additions without purchaser consent are prohibited except to finish the heat; residuals may be present but must not impair properties. ; Table 2, note b permits specified deviations where hardenability is required, except for P/S; The default composition range is not widened here. ; Mechanical properties, delivery and hardenability require separate verification; suitability for forming a specific component requires separate confirmation.
Verification notes
Older-edition Tables 2 and 3 and footnotes visually checked; equivalence to the newer edition is not assumed.42CrMoS4 · EN 10263-4-2001
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- EN 10263-4-2001
- Table / clause
- Table 2
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | ≤ 0.3 (lower limit not stated) |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cu | ≤ 0.25 (lower limit not stated) |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
DIN EN10263-4:2002-02 adopts EN10263-4:2001; the edition relationship is expressly identified on the cover; Heat-analysis mass percentages. ; Historical Table 2/3 contains no optional Al addition note for 2017; newer-edition conditions are not applied. ; Table 2, note c permits an agreed carbon range of width .04%; tabulated defaults are unchanged without a specific agreement. ; Table 2, note d and Table 3, note c permit agreed lower Si, considering effects on properties/hardenability; no range is invented where none is specified. ; Unlisted elements are not entered as zero; Table 2, note a: intentional additions without purchaser consent are prohibited except to finish the heat; residuals may be present but must not impair properties. ; Table 2, note b permits specified deviations where hardenability is required, except for P/S; The default composition range is not widened here. ; Mechanical properties, delivery and hardenability require separate verification; suitability for forming a specific component requires separate confirmation.
Verification notes
Older-edition Tables 2 and 3 and footnotes visually checked; equivalence to the newer edition is not assumed.42CrMoS4 · DIN EN 10083-3-2007
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- DIN EN 10083-3-2007
- Table / clause
- Table 3 · Notes a–c
- PDF page references
- 1、18
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Mn | 0.6 ~ 0.9 |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Si | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.025 (lower limit not stated) |
Applicability and limitations
Composition is based on Table 3 of EN10083-3:2006 in the official English text of DIN EN10083-3:2007-01, heat analysis wt%. ; Note a: Elements not listed shall not be intentionally added without the purchaser's consent, except for additions needed to finish steelmaking and to enable boron to act on hardenability.; Unspecified values shall not be treated as zero. ; Note b: Small deviations are permitted where hardenability or quenched-and-tempered mechanical-property requirements apply, except for C/P/S; permitted deviations for other elements must not exceed Table 4.; Default heat analysis range shall not be expanded. ; For non-boron steels in this standard, Note c permits steel with improved machinability to be supplied on request: sulfur approximately 0.10%, with the Mn upper limit permitted to increase by an absolute 0.15%.; Approximate values are not default hard upper limits and must be determined by specific inquiry/order; they shall not be automatically mixed with ordinary grades. ; This standard covers alloy steels for quenching and tempering. Suitability for cold heading, wire-rod supply, annealing, surface and dimensions require separate confirmation; do not automatically add products..
Verification notes
Official English source cover, all 28 grades in Table 3 and notes a–c visually checked.Permitted product-analysis deviations (must not be added to heat-analysis limits)
DIN EN10083-3:2007-01 (adopting EN10083-3:2006) · Table 4 and notes a/b, 7.1.2.2; Product analysis specified at ordering follows A.5 · PDF pages 11, 19, 55 · mass fraction wt%; Deviations are expressed in percentage points of mass percentage
The complete standard tolerance table applies only to elements specified in the original table for this grade and to the corresponding content/sulfur-range conditions; it does not widen heat-analysis composition, carbon equivalent or reverse-search ranges.
| Element | Specified maximum heat-analysis content, wt% | Lower deviation, percentage points | Upper deviation, percentage points | Applicable conditions |
|---|---|---|---|---|
| C | ≤0.55 | -0.02 | +0.02 | Select the cast-analysis maximum-content band specified in the original table |
| Si | ≤0.40 | The original table does not state a negative deviation | +0.03 | Select the cast-analysis maximum-content band specified in the original table |
| Mn | ≤1.00 | -0.04 | +0.04 | Select the cast-analysis maximum-content band specified in the original table |
| Mn | >1.00≤1.70 | -0.05 | +0.05 | Select the cast-analysis maximum-content band specified in the original table |
| P | ≤0.025 | The original table does not state a negative deviation | +0.005 | Select the cast-analysis maximum-content band specified in the original table |
| S | ≤0.040 | The original table does not state a negative deviation | +0.005 | Only the sulfur upper limit is specified; Note b’s full 0.020–0.040% range is not applied. |
| Cr | ≤2.00 | -0.05 | +0.05 | Select the cast-analysis maximum-content band specified in the original table |
| Cr | >2.00≤2.20 | -0.1 | +0.1 | Select the cast-analysis maximum-content band specified in the original table |
| Mo | ≤0.30 | -0.03 | +0.03 | Select the cast-analysis maximum-content band specified in the original table |
| Mo | >0.30≤0.60 | -0.04 | +0.04 | Select the cast-analysis maximum-content band specified in the original table |
| Ni | ≤2.00 | -0.05 | +0.05 | Select the cast-analysis maximum-content band specified in the original table |
| Ni | >2.00≤4.3 | -0.07 | +0.07 | Select the cast-analysis maximum-content band specified in the original table |
| V | ≤0.25 | -0.02 | +0.02 | Select the cast-analysis maximum-content band specified in the original table |
| B | ≤0.0050 | -0.0003 | +0.0003 | Select the cast-analysis maximum-content band specified in the original table |
| S | ≤0.040 | -0.005 | +0.005 | Only when Table 3 heat analysis explicitly specifies the full S range of 0.020–0.040% (Table 4, Note b). |
- Table 4 Note a: For a same-heat tolerance, deviation is permitted in only one direction—above the upper limit or below the lower limit—not both.
- S product-analysis tolerance is usually only +0.005. Note b permits ±0.005 only for steels whose heat analysis explicitly specifies the full 0.020–0.040% range; do not apply Note b based only on the maximum S value.
- Clause 7.1.2.2 requires product analysis to be specified at ordering and refers to A.5; without a heat-lot test report, this table does not prove that the actual product conforms.
- A.5: one product analysis per heat, limited to elements specified for the grade; sampling per EN ISO 14284. For disputes, reference methods are the European standards listed in CR 10261.
This is a complete standard deviation table and does not imply that every element for this grade is specified; Elements not listed are not added on the basis of this table. Symmetric deviation for the same heat is permitted in only one direction, either upward or downward; Asymmetric deviation for Pb is only found in the Pb row of EN10087 and cannot be applied to other standards where Pb is not listed. Do not automatically expand heat analysis composition, carbon equivalent, or reverse-lookup ranges.
42CrMoS4 · EN 10083-3-2006
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- EN 10083-3-2006
- Table / clause
- Table 3 · Notes a–c
- PDF page references
- 1、18
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Mn | 0.6 ~ 0.9 |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Si | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.025 (lower limit not stated) |
Applicability and limitations
Composition is based on Table 3 of EN10083-3:2006 in the official English text of DIN EN10083-3:2007-01, heat analysis wt%. ; Note a: Elements not listed shall not be intentionally added without the purchaser's consent, except for additions needed to finish steelmaking and to enable boron to act on hardenability.; Unspecified values shall not be treated as zero. ; Note b: Small deviations are permitted where hardenability or quenched-and-tempered mechanical-property requirements apply, except for C/P/S; permitted deviations for other elements must not exceed Table 4.; Default heat analysis range shall not be expanded. ; For non-boron steels in this standard, Note c permits steel with improved machinability to be supplied on request: sulfur approximately 0.10%, with the Mn upper limit permitted to increase by an absolute 0.15%.; Approximate values are not default hard upper limits and must be determined by specific inquiry/order; they shall not be automatically mixed with ordinary grades. ; This standard covers alloy steels for quenching and tempering. Suitability for cold heading, wire-rod supply, annealing, surface and dimensions require separate confirmation; do not automatically add products..
Verification notes
Official English source cover, all 28 grades in Table 3 and notes a–c visually checked.42CrMoS4 · NF EN 10083-3-2006
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Composition basis in the adopted standard verified
- Standard edition
- EN 10083-3-2006
- Table / clause
- Table 3 · Notes a–c
- PDF page references
- 1、18
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Mn | 0.6 ~ 0.9 |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Si | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.025 (lower limit not stated) |
Applicability and limitations
NF EN 10083-3:2006-12 corresponds to EN 10083-3:2006; Composition is read from the verified official original text of this EN version; see Data Basis for the actual source document. Composition is based on Table 3 of EN10083-3:2006 in the official English text of DIN EN10083-3:2007-01, heat analysis wt%. ; Note a: Elements not listed shall not be intentionally added without the purchaser's consent, except for additions needed to finish steelmaking and to enable boron to act on hardenability.; Unspecified values shall not be treated as zero. ; Note b: Small deviations are permitted where hardenability or quenched-and-tempered mechanical-property requirements apply, except for C/P/S; permitted deviations for other elements must not exceed Table 4.; Default heat analysis range shall not be expanded. ; For non-boron steels in this standard, Note c permits steel with improved machinability to be supplied on request: sulfur approximately 0.10%, with the Mn upper limit permitted to increase by an absolute 0.15%.; Approximate values are not default hard upper limits and must be determined by specific inquiry/order; they shall not be automatically mixed with ordinary grades. ; This standard covers alloy steels for quenching and tempering. Suitability for cold heading, wire-rod supply, annealing, surface and dimensions require separate confirmation; do not automatically add products..
Verification notes
The adoption relationship and original corresponding EN composition table have been checked; The complete main text of NF has not been checked page by page42CrMoS4 · DIN 17200-1987
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Alloy steel
- Subcategory
- Alloy steel
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- DIN 17200-1987-03
- Table / clause
- Table 2 and footnotes 1–5; 7.3.1–7.3.2
- PDF page references
- 1、2、15、16、17
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Mn | 0.6 ~ 0.9 |
| S | 0.02 ~ 0.035 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Si | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.035 (lower limit not stated) |
Applicability and limitations
Table 2 cast analysis, mass fraction wt%; Si is an upper limit and unspecified elements are not filled with zero. P/S requirements for the C, Ck and Cm series remain separate; S 0.020–0.035% in S-containing grades is a two-sided range. Note 1: unlisted elements may not be intentionally added without purchaser consent, except to complete melting; no fixed residual values are inferred. Table 3 contains permissible product-analysis deviations, not added to cast limits; applicable sizes and positive/negative directions are checked separately. Heat-treatment condition, hardenability and size-dependent properties require separate verification. The standard includes hot-rolled wire rod; chemistry alone is no cold-heading supply commitment. Note 2: small composition deviations, excluding P/S, may be agreed when ordering restricted hardenability bands or quenched-and-tempered/normalized properties, but may not exceed Table 3. These data retain the Table 2 baseline without automatic relaxation. Light-typeface grades in note 4 are for special applications only. Note 5 permits separate ordering of Pb 0.15–0.30% only for the marked C-series grades; not added to ordinary base compositions. Original material number 1.7227; not marked for special application under note 4.
Verification notes
March 1987, Table 2 and all footnotes transcribed; mechanical properties checked separately.42CrMoS4 · EN ISO 683-2-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Alloy steel
- Subcategory
- Alloy steel for quenching and tempering
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- EN ISO 683-2-2018
- Table / clause
- Table 3, notes a–d; clause 7.1.2; Table 4 limits
- PDF page references
- 22
- Unit
- Mass fraction (wt%)
- Analysis type
- Heat analysis; not product analysis
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | 0.1 ~ 0.4 |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Cu | ≤ 0.4 (lower limit not stated) |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
Table 3 herein applies to heat (cast) analysis, mass fraction wt%; The permissible deviations for product analysis in Table 4 shall not be directly added to the limits in general Table 3. This document is EN ISO 683-2:2018, adopted without modification and accompanied by the text of ISO 683-2:2016; This record explicitly preserves the identity of EN ISO 683-2-2018 and shall not be called the ISO 2018 edition. Only the chemical composition and source conditions of Table 3 are verified; this does not constitute a guarantee of hardenability, heat treatment, mechanical properties, wire delivery state, or cold heading process. Note a: deviations in heat analysis apply only when hardenability requirements are specified; The deviation in C shall not exceed ±0.01%; P/S is excluded, and the other elements follow Table 4. General Table 3 shall not be automatically relaxed, nor shall H/HH/HL be merged with general grades. Note b: Steel with S increased to approximately 0.10% (including sulfide morphology control) or with the addition of Pb to improve machinability may be requested from the supplier; When S is increased, the upper limit of Mn may be increased by 0.15 percentage points. This agreement is not a default requirement, and approximate values shall not serve as precise automatic limits for this batch; if the Pb range is not listed, values shall not be borrowed from other standards. Original Note: Elements not listed shall not be intentionally added without the consent of the purchaser, except those required to complete the melting process; Elements introduced via scrap steel etc. shall be controlled. An unlisted value must not be assumed to be zero. Note d: lower Si is permitted, but other deoxidation methods must be used; The original text does not provide a uniform lower Si range; agreed conditions shall not automatically replace the range listed in 0.10–0.40%. This line is an independent S grade, S 0.020–0.040%, and shall not be merged with the S upper limit of grades without the S designation.
Verification notes
Original-image verification of all 25 physical rows and merged cells in Table 3; reuse existing independently cropped evidence for 5 same-source rows and 40 cells, transcribe the remaining cells individually from the source images, and record the two editions separately.42CrMoS4 · ISO 683-2-2016
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Alloy steel
- Subcategory
- Alloy steel for quenching and tempering
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 683-2-2016
- Table / clause
- Table 3, notes a–d; clause 7.1.2; Table 4 limits
- PDF page references
- 22
- Unit
- Mass fraction (wt%)
- Analysis type
- Heat analysis; not product analysis
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | 0.1 ~ 0.4 |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Cu | ≤ 0.4 (lower limit not stated) |
| Mo | 0.15 ~ 0.3 |
Applicability and limitations
Table 3 herein applies to heat (cast) analysis, mass fraction wt%; The permissible deviations for product analysis in Table 4 shall not be directly added to the limits in general Table 3. This document is EN ISO 683-2:2018, adopted without modification and accompanied by the text of ISO 683-2:2016; This record explicitly preserves the identity of ISO 683-2-2016 and shall not be called the ISO 2018 edition. Only the chemical composition and source conditions of Table 3 are verified; this does not constitute a guarantee of hardenability, heat treatment, mechanical properties, wire delivery state, or cold heading process. Note a: deviations in heat analysis apply only when hardenability requirements are specified; The deviation in C shall not exceed ±0.01%; P/S is excluded, and the other elements follow Table 4. General Table 3 shall not be automatically relaxed, nor shall H/HH/HL be merged with general grades. Note b: Steel with S increased to approximately 0.10% (including sulfide morphology control) or with the addition of Pb to improve machinability may be requested from the supplier; When S is increased, the upper limit of Mn may be increased by 0.15 percentage points. This agreement is not a default requirement, and approximate values shall not serve as precise automatic limits for this batch; if the Pb range is not listed, values shall not be borrowed from other standards. Original Note: Elements not listed shall not be intentionally added without the consent of the purchaser, except those required to complete the melting process; Elements introduced via scrap steel etc. shall be controlled. An unlisted value must not be assumed to be zero. Note d: lower Si is permitted, but other deoxidation methods must be used; The original text does not provide a uniform lower Si range; agreed conditions shall not automatically replace the range listed in 0.10–0.40%. This line is an independent S grade, S 0.020–0.040%, and shall not be merged with the S upper limit of grades without the S designation.
Verification notes
Original-image verification of all 25 physical rows and merged cells in Table 3; reuse existing independently cropped evidence for 5 same-source rows and 40 cells, transcribe the remaining cells individually from the source images, and record the two editions separately.42CrMoS4 · EN 10263
Original-source verification is incomplete; this is not a formal standard reference
- Material form
- Drawn wire
- Verification status
- Published on the website; original-source verification pending
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Cr | 0.9 ~ 1.2 |
| Mn | 0.6 ~ 0.9 |
| Mo | 0.15 ~ 0.3 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Si | ≤ 0.4 (lower limit not stated) |
Applicability and limitations
Give priority to the published technical page on the Creation Group website. Use local reference ranges only as supplementary composition cross-checks; the applicable standard for that product page, the technical agreement and actual verification take precedence.
42CrMoS4 · JIS G 7105-2000
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Alloy steel
- Subcategory
- Alloy steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Cr | 0.9 ~ 1.2 |
| Mn | 0.6 ~ 0.9 |
| Mo | 0.15 ~ 0.3 |
| P | ≤ 0.035 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
42CrMoS4 · DIN EN 10277:2018-09
Original table in an informative annex verified; normative composition requirements and edition still require verification. For reference only.
- Material category
- Alloy steel
- Subcategory
- Alloy steel
- Material form
- Reference record
- Composition basis
- Heat analysis in an informative annex; for reference only
- Verification status
- Original table in an informative annex verified; normative composition requirements and edition still require verification
- Standard edition
- DIN EN 10277:2018-09
- Table / clause
- Informative Annex A.4
- PDF page references
- 47
- Unit
- mass fraction (wt%)
- Analysis type
- Heat analysis (informative reference)
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.38 ~ 0.45 |
| Si | 0.1 ~ 0.4 |
| Mn | 0.6 ~ 0.9 |
| P | ≤ 0.025 (lower limit not stated) |
| S | 0.02 ~ 0.04 |
| Cr | 0.9 ~ 1.2 |
| Mo | 0.15 ~ 0.3 |
| Cu | ≤ 0.4 (lower limit not stated) |
Applicability and limitations
The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
Composition conditions
- The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
- Footnote b: A quotation is required to raise S to about 0.10% or add Pb; when S is increased, the Mn upper limit may be raised by 0.15%, but this is not automatic.
- Footnote c: Reducing Si requires other deoxidation measures.
- Unlisted elements shall not be intentionally added without the buyer’s consent.
Conditional requirement
- Footnote
- Informative boundary
- Source conditions
- The original informative annex table has been checked and is for reference only; Main-text 7.1.2 requires chemical composition to be determined under the referenced standards; the normative composition and applicable editions still require verification. It must not be used as a delivery guarantee, reverse-matching criterion or basis for carbon equivalent calculated from standard composition ranges. Main-text references: EN ISO 683-1 and EN ISO 683-2 (undated references; applicable editions awaiting verification).
- Footnote
- Original-table condition 1
- Source conditions
- Footnote b: A quotation is required to raise S to about 0.10% or add Pb; when S is increased, the Mn upper limit may be raised by 0.15%, but this is not automatic.
- Footnote
- Original-table condition 2
- Source conditions
- Footnote c: Reducing Si requires other deoxidation measures.
- Footnote
- Original-table condition 3
- Source conditions
- Unlisted elements shall not be intentionally added without the buyer’s consent.