Products/ISO 4954

MATERIAL DATA · COLD FORMING

33B2 CHQ wire

Reference technical data for 33B2. Source edition: ISO 4954:2018 · Annex C. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

33B2 CHQ wire product image
33B2 · Cold heading wire
01Applicable standardISO 4954:2018 · Annex C
02Material grade33B2
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

33B2 · ISO 4954:2018

33B2 · ISO 4954:2018 · Mass fraction / %
ElementMass fraction / %
C0.3–0.35
Si≤0.3
Mn0.6–0.9
P≤0.025
S≤0.025
Cr≤0.3
B0.0008–0.005
Cu≤0.25
Source: ISO 4954:2018
Composition source and applicability · ISO 4954:2018 · PDF 24
ISO 4954:2018 · PDF 24
Composition source and applicability · ISO 4954:2018 · PDF 29
ISO 4954:2018 · PDF 29
Composition source and applicability · ISO 4954:2018 · PDF 30
ISO 4954:2018 · PDF 30
Composition source and applicability · ISO 4954:2018 · PDF 41
ISO 4954:2018 · PDF 41
Composition source and applicability · ISO 4954:2018 · PDF 43
ISO 4954:2018 · PDF 43
Composition source and applicability · ISO 4954:2018 · PDF 44
ISO 4954:2018 · PDF 44
Composition source and applicability · ISO 4954:2018 · PDF 58
ISO 4954:2018 · PDF 58
Composition source and applicability · ISO 4954:2018 · PDF 59
ISO 4954:2018 · PDF 59
Composition source and applicability · ISO 4954:2018 · PDF 60
ISO 4954:2018 · PDF 60

1. Delivery conditions and applicable requirements

Table C.1 – Combinations of heat-treatment condition at delivery, product form and applicable requirements

Delivery conditionSymbolWire rodBarWire
Hot rolled or peeled+AR or +PEXXX
Cold drawn+AR+C—XX
Cold drawn and spheroidize annealed+AR+C+AC—XX
Cold drawn, spheroidize annealed and lightly cold drawn+AR+C+AC+LC—XX
Spheroidize annealed or spheroidize annealed and peeled+AC or +AC+PEXXX
Spheroidize annealed and cold drawn+AC+C—XX
Spheroidize annealed, cold drawn and spheroidize annealed again+AC+C+AC—XX
Spheroidize annealed, cold drawn, spheroidize annealed again and lightly cold drawn+AC+C+AC+LC—XX

X = applicable; — = not applicable.

Other delivery conditions may be agreed at the time of order.

Applicable requirements according to the basis of order

Ordered with reference to steel names in the tablesRequirement
C.2, C.3, C.4, C.5 or C.6Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6.
C.2, C.3, C.4, C.5, C.6, C.7, C.8 or C.9Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; hardenability values according to C.7, C.8 and C.9.
C.2, C.3, C.4, C.5, C.6 or C.10Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; minimum core hardness and maximum diameter according to C.10.

Supplementary or special requirements under Annex E apply if agreed at the time of enquiry and order.

Source: ISO 4954:2018, Table C.1, page 34. This table gives the standard relationship between product form, delivery condition and requirements; actual supply must be confirmed separately.

2. Chemical composition

Table C.3 – Chemical composition of boron-alloyed steels for quenching and tempering (cast analysis)

These are the standard’s reference requirements for cast analysis of 33B2, not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials of elements that could impair hardenability, mechanical properties or suitability.

Al of 0.020–0.050% may be added to improve cold-heading performance.

a: Single values are maximum limits unless otherwise indicated. A dash does not mean zero content.

b: For steels with hardenability requirements under Table C.8, small departures from the specified limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 2 for the other elements.

c: A lower silicon content may be agreed at the time of order. Its effects on the specified properties, such as hardenability, must then be assessed.

d: Where a maximum chromium content of 0.30% is specified, a lower limit may also be agreed at the time of enquiry and order.

e: To achieve through-hardening to the core for 30MoB1, the lower Cr limit shall be 0.15% and may be agreed at the time of enquiry and order. For particular applications, a lower upper Cr limit may also be agreed at the time of enquiry and order.

Source: ISO 4954:2018, Table C.3, page 37 (PDF page 43). The table and notes do not replace the complete standard.

3. Mechanical properties

Table C.6 – Mechanical properties of boron-alloyed steels

Steel nameDiameterDelivery condition
+AR or +PE+AC or +AC+PE+AR+C+AR+C+AC+AR+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
33B225——————5406458062——
33B2510——55062——530645706264057
33B21040——55062——530645706263057

The tensile-strength values in delivery condition +AR are not compatible with the entire composition range for a steel grade in Table C.3. Compatibility between tensile-strength values and hardenability requirements must be checked for the supplied diameter and composition.

Source: ISO 4954:2018, Table C.6, page 41. Rm is tensile strength; Z is reduction of area at fracture. The values apply only to the specified diameter intervals and delivery conditions.

4. Hardenability requirements

Table C.8 – Hardness limits for boron-alloyed steels with specified normal hardenability (+H)

Steel nameSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
33B2+H870max.555554524943—————————
33B2+H870min.4945432720——————————

Source: ISO 4954:2018, Table C.8, page 46.

Table C.10 – Minimum core hardness and maximum diameter for at least 90% martensite in the core-hardening test (+CH)

Steel nameSymbolAustenitizing temperature, °C (±5 °C), see note aMinimum core hardness, HRCMaximum diameter, mm, see note b
33B2+CH8704511

a: As a guide, a holding time of at least 30 minutes at the hardening temperature is recommended.

b: The specified maximum diameters are achievable at the lowest hardenability within each steel grade. For +HH qualities, the maximum diameter may be increased.

Source: ISO 4954:2018, Table C.10, page 50.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 33B2

Basis: ISO 4954

Chemical composition source: ISO 4954:2018

Transcribed from the cited standard

The technical data and chemical composition on this page cite ISO 4954:2018. Confirm the applicable contract edition separately; do not assume other editions are identical.

Original source wording

Table C.3

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.4000–0.5767

Missing elements: Mo, V, Ni

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.3340–0.4575

Missing elements: Ni, Mo, V

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.3600–0.4675

Missing elements: Mo, Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group