Products/EN 10263

MATERIAL DATA · COLD FORMING

25CrMoS4 Cold-drawn steel wire

Reference technical data for 25CrMoS4. Source edition: EN 10263-4:2017. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

25CrMoS4 Cold-drawn steel wire product image
25CrMoS4 · Cold-drawn steel wire
01Applicable standardEN 10263-4:2017
02Material grade25CrMoS4
03Product formCold-drawn steel wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Delivery conditions and applicable requirements

Table 1 – Delivery conditions, product forms and applicable requirements

Heat-treatment conditionSymbolBarWire rodWire
UntreatedNone or +UXX—
Spheroidize annealed+ACXXX
Basis of orderApplicable requirements
Table 3 and 4, 6 or 7 or 8Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8.
Table 3 and 4, 6 or 7 or 8, 9 or 10 or 11Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8; hardenability according to Table 9, 10 or 11.
Table 3 and 4, 6 or 7 or 8, 12Chemical composition according to Tables 3 and 4; mechanical properties according to Table 6, 7 or 8; minimum core hardness and maximum diameter according to Table 12.
Table 3, 4, 6, 7, 8, 9, 10, 11 or 12Supplementary or special requirements under Annex A of EN 10263-1, if agreed at the time of enquiry and order.

Table 2 – Surface condition at delivery

Basis of agreementSurface conditionSymbolBarWire rodWire
Unless otherwise agreedAs rolledNone or +ARXX—
Special surface condition by agreementCold drawn+C——X
Special surface condition by agreementLightly cold drawn+LCX—X
Special surface condition by agreementPeeled+PEXXX

X = applicable; — = not applicable. Other delivery conditions may be agreed at the time of order.

Heat-treatment condition and surface condition are separate requirements. This table gives the standard reference; the actual product form, delivery condition and suitability must be confirmed in the order.

Source: EN 10263-4:2017, Table 1 and 2, page 6–7 (PDF page 7–8).

2. Chemical composition

Table 3 – Chemical composition of steels without boron (cast analysis)

Reference requirements for 25CrMoS4, steel number 1.7213. These are not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

ElementMass fraction, %
C0.22–0.29
Si≤0.30
Mn0.60–0.90
P≤0.025
S0.020–0.040
Cr0.90–1.20
Mo0.15–0.30
Ni—
Cu≤0.25

Values are mass fractions in percent. Single values are maximum limits unless otherwise indicated. “—” represents a blank source field and does not mean zero content.

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials that could impair hardenability, mechanical properties or suitability.

For steels with hardenability requirements under Tables 9–11, small departures from the composition limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 5 for the other elements.

An aluminium addition of 0.020–0.050% is possible to improve cold-heading performance.

A lower silicon content may be agreed at the time of order. Its effect on the specified properties, such as hardenability, must be assessed.

A carbon range 0.04 percentage points wide, for example 0.33–0.37%, may be agreed at the time of enquiry and order.

Table 5 – Permissible deviations for product analysis

ElementLimiting values for cast analysis, %Permissible deviation for product analysis, %
C≤0.50±0.02
Si≤0.30±0.03
Mn≤1.00±0.04
Mn>1.00 and ≤1.45±0.05
P≤0.025+0.005
S≤0.025+0.005
Cr≤1.70±0.05
Mo≤0.30±0.03
Ni≤2.00±0.05
B≤0.0050±0.0003
Cu≤0.25+0.03

± means that, within one heat, the product analysis for an element may deviate above the upper limit or below the lower limit in Tables 3 and 4, but not in both directions at the same time.

For steels with a specified sulfur range of 0.020–0.035% or 0.020–0.040% in the cast analysis, the permissible deviation is ±0.005%.

Source: EN 10263-4:2017, Table 3 on page 8 (PDF page 9), and Table 5 on page 10 (PDF page 11). These tables do not replace the complete standard.

3. Mechanical properties

Table 7 – Mechanical properties of alloy steels without boron in the specified delivery condition

Steel nameSteel numberDiameterDelivery condition
+AC or +AC+PE+AC+C+AC+AC+C+AC+LC
over, mmup to and including, mmRm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
25CrMoS41.721325——5706261060
25CrMoS41.7213540580605606260060

Source: EN 10263-4:2017, Table 7, page 11. Rm is tensile strength; Z is reduction of area at fracture. The values apply to the specified diameter intervals and delivery conditions. A dash does not mean zero or confirm availability.

4. Hardenability requirements

Table 9 – Hardness limits for steels without boron with normal hardenability (+H)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
25CrMoS41.7213+H850max.525251504846434137353332313131
25CrMoS41.7213+H850min.4443403734322927232120————

Source: EN 10263-4:2017, Table 9, page 15.

Table 10 – Hardness limits for steels without boron with restricted hardenability bands (+HH and +HL)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.5357911131520253035404550
25CrMoS41.7213+HH850max.525251504846434137353332313131
25CrMoS41.7213+HH850min.474644413937343228262423222222
25CrMoS41.7213+HL850max.494947464341383632302928272727
25CrMoS41.7213+HL850min.4443403734322927232120————

Table 10 does not apply to steels ordered with a restricted carbon range under note b to Table 3.

Source: EN 10263-4:2017, Table 10, page 18.

Table 12 – Maximum diameter for at least 90% martensite in the core-hardening test (+CH)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C), see note aMinimum core hardness, HRCMaximum diameter, mm, see note b
25CrMoS41.7213+CH8504113

As a guide, a holding time of at least 30 minutes at the specified hardening temperature is recommended.

The maximum diameters apply to the lowest hardenability within each steel grade. For +HH qualities, the maximum diameter may be increased.

Source: EN 10263-4:2017, Table 12, page 21.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 25CrMoS4

Basis: EN 10263

Chemical composition source: BS EN 10263-4:2017

Transcribed from the cited standard

Original source wording

Table 3

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.5300–0.7567

Missing elements: V, Ni

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.3050–0.4375

Missing elements: Ni, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.3400–0.4825

Missing elements: Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →