Products/GB/T 5953

MATERIAL DATA · COLD FORMING

ML20Mn Cold heading wire

Technical data for ML20Mn Cold heading wire, compliant with GB/T 5953. View the chemical composition, mechanical properties, and related technical requirements for this grade.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

ML20Mn Cold heading wire
ML20Mn · Cold heading wire
01Applicable standardGB/T 5953
02Material gradeML20Mn
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

ML20Mn · GB/T 6478-2015

ML20Mn · GB/T 6478-2015 · Mass fraction / %
ElementMass fraction / %
C0.18~0.23
Si≤0.10
Mn0.70~1.00
P≤0.030
S≤0.035
Ni≤0.20
Cr≤0.20
Cu≤0.20
Al(total)≥0.020
Source: GB/T 6478-2015
Composition source and applicability · GB/T 6478-2015 · PDF 8
GB/T 6478-2015 · PDF 8
Composition source and applicability · GB/T 6478-2015 · PDF 9
GB/T 6478-2015 · PDF 9
Composition source and applicability · GB/T 6478-2015 · PDF 10
GB/T 6478-2015 · PDF 10

1. Chemical Composition

Composition source and applicability

Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.

Source: GB/T 6478-2015 · ML20Mn · p.8

2. Mechanical Properties

Table 2 Mechanical properties of surface-hardening steel wire

Grade a)Diameter/mmBALANCESA
Tensile strength Rm/MPaReduction of area Z / %Rockwell hardness/HRBTensile strength Rm/MPaReduction of area Z / %Rockwell hardness/HRB
ML20Mn ML16CrMn ML20MnA ML22Mn ML15Cr ML20Cr ML18CrMo≤6.00440-640≥55-370-520≥60≤82
>6.00 - 12.00420-600≥55-
>12.00-25.00400-550≥50≤85
Note: The reduction of area for wire with a diameter less than 3.00 mm is for reference only.
a) The chemical composition of grades may refer to GB/T 6478.

2.1 For wire delivered in the HD condition, mechanical properties shall be determined by agreement between the supplier and the purchaser.
2.2 The mechanical properties of surface-hardening steel wire in the delivery condition shall comply with the requirements specified in Table 2.
2.3 When wire is delivered in straight lengths or in a polished condition, a 10% variation in mechanical properties is permitted.
2.4 For wire with a nominal diameter greater than 25.00 mm, the mechanical properties shall be determined by agreement between the supplier and the purchaser.
2.5 The mechanical properties for grades not listed in the table shall be determined by agreement between the supplier and the purchaser.
2.6 Upsetting: Wire samples shall be cold upset to one-half of their original height without surface cracks or fissures. By mutual agreement, upsetting may also be performed to one-third or one-quarter of the original sample height.

3. Microstructure

Table 6 Permissible range for decarburized layer depth

For spheroidizing annealed wire, the spheroidized microstructure may be inspected upon the purchaser's request and as specified in the contract; the acceptance criteria and test methods shall be agreed upon by the supplier and the purchaser.

Nominal diameter of wireDepth of complete decarburizationTotal decarburized layer depth
≤8.00≤0.02≤0.10
>8.00-15.0≤0.02≤0.15
>15.0-25.0≤0.03≤0.20
>25.0-45.0By agreementBy agreement

3.1 Decarburized layer: Upon the purchaser's request and as specified in the contract, the decarburized layer on the wire surface may be inspected. The permissible depth of the total decarburized layer (ferrite + transition zone) and the complete decarburized layer on one side shall comply with Table 6. Special requirements for the decarburized layer shall be determined by agreement between the supplier and the purchaser. For wire grades with a carbon content not greater than 0.30%, the test method shall be agreed upon by the supplier and the purchaser.
3.2 Carburization: The wire surface shall be free from carburization. Inspection may be omitted if the supplier can provide assurance.

4. Surface quality


4.1 The wire surface shall be smooth and free from cracks, scabs, folds, laminations, drawing marks, and rust. However, individual pits, raised surfaces, indentations, and scratches with a depth not exceeding half the diameter tolerance are permitted. Wire delivered in the annealed condition may exhibit oxidation colors on the surface.
4.2 Requirements for wire surface coatings shall be determined by mutual agreement between the supplier and the purchaser.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — ML20Mn

Basis: GB/T 5953

Chemical composition source: GB/T 6478-2015

Transcribed from the cited standard

Original source wording

Table 2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.2967–0.4633

Missing elements: Mo, V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.2150–0.3067

Missing elements: Mo, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.2500–0.3550

Missing elements: Mo

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group