Products/EN 10263

MATERIAL DATA · COLD FORMING

C8C Cold-drawn steel wire

Reference technical data for C8C. Source edition: EN 10263-2:2017. Read chemistry, delivery conditions and properties with their cited limits and notes. The applicable edition and acceptance requirements must be confirmed in the order technical agreement.

Supply and technical review · Creation Group accepts supply and technical review enquiries for this product. Dimensions, delivery condition, quantity and inspection documents are confirmed in the order technical agreement after review.

C8C Cold-drawn steel wire product image
C8C · Cold-drawn steel wire
01Applicable standardEN 10263-2:2017
02Material gradeC8C
03Product formCold-drawn steel wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Delivery conditions and applicable requirements

Table 1 – Delivery conditions, product forms and applicable requirements

Delivery conditionSymbolWire rodBarWire
As hot rolled+UXX—
Peeled+U+PEXX—
Cold drawn+U+C—XX
Cold drawn and spheroidize annealed+U+C+AC—XX
Cold drawn, spheroidize annealed and lightly drawn+U+C+AC+LC—XX
Annealed to achieve spheroidal carbides, possibly followed by peeling+AC or +AC+PEXX—
Annealed to achieve spheroidal carbides and then cold drawn+AC+C—XX
Basis of orderApplicable requirements
Chemical compositionTable 2 and 3
Mechanical propertiesTable 4
Supplementary or special requirementsAnnex A of EN 10263-1, if agreed at the time of enquiry and order.

X = applicable; — = not applicable. Other delivery conditions may be agreed at the time of order.

This table gives the standard combinations of product form and delivery condition. Actual supply and suitability require technical assessment.

Source: EN 10263-2:2017, Table 1, page 6 (PDF page 8).

2. Chemical composition

Table 2 – Chemical composition of steels not intended for heat treatment after cold working (cast analysis)

Reference requirements for C8C, steel number 1.0213. These are not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

ElementMass fraction, %
C0.06–0.10
Si≤0.10
Mn0.25–0.45
P≤0.020
S≤0.025
Al0.020–0.060

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other raw materials. Residual elements may be present if they do not impair mechanical properties or suitability.

Aluminium may be replaced by one or more elements with a similar effect.

Table 3 – Permissible deviations for product analysis

ElementLimiting values for cast analysis, %Permissible deviation for product analysis, %
C≤0.22±0.02
Si≤1.00+0.03
Si>1.00±0.05
Mn≤1.00±0.04
Mn>1.00 and ≤1.80±0.05
P≤0.025+0.005
S≤0.025+0.005
Al≤0.060±0.005

± means that, within one heat, the product analysis for a given element may deviate above the upper limit or below the lower limit in Table 2, but not both at the same time.

Source: EN 10263-2:2017, Table 2 on page 7 (PDF page 9), and Table 3 on page 8 (PDF page 10). These tables do not replace the complete standard.

3. Mechanical properties

Table 4 – Mechanical properties of steels not intended for heat treatment after cold working, in the specified delivery condition

Steel nameSteel numberDiameterDelivery condition
+U or +U+PE+AC or +AC+PE+U+C+U+C+AC+U+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
C8C1.021325——————3507239068——
C8C1.0213510410653607049063340723806845065
C8C1.02131040410653607048063340723806844065
C8C1.0213401004106536070————————

Note a: Z values for +U or +U+PE are given for information only.

Note b: The marked Rm values for 8MnSi7 and 7MnB8 are minimum values, although the column heading specifies maximum.

Note c: The standard states that a particular application of 7MnB8 is patented. This is a statement in the 2017 source, not an assessment of current patent status.

Source: EN 10263-2:2017, Table 4, page 9. Rm is tensile strength; Z is reduction of area at fracture. The values apply to the specified diameter intervals and delivery conditions. A dash does not mean zero or confirm availability.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — C8C

Basis: EN 10263

Chemical composition source: BS EN 10263-2:2017

Transcribed from the cited standard

Original source wording

Table 2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.1017–0.1750

Missing elements: Cr, Mo, V, Ni, Cu

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.0725–0.1258

Missing elements: Cu, Cr, Ni, Mo, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.0850–0.1450

Missing elements: Mo, Cr, Cu, Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group