01Applicable standardISO 4954:2018 · Annex B
02Material gradeC10E2C
03Product formCold heading wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Delivery conditions and applicable requirements

Table B.1 – Combinations of heat-treatment condition at delivery, product form and applicable requirements

Delivery conditionSymbolWire rodBarWire
Hot rolled or peeled+AR or +PEXXX
Cold drawn+AR+C—XX
Cold drawn and spheroidize annealed+AR+C+AC—XX
Cold drawn, spheroidize annealed and lightly cold drawn+AR+C+AC+LC—XX
Spheroidize annealed or spheroidize annealed and peeled+AC or +AC+PEXXX
Spheroidize annealed and cold drawn+AC+C—XX
Treated to a ferrite-pearlite structure and specified hardness range+FP—X—

X = applicable; — = not applicable.

Other delivery conditions may be agreed at the time of order.

Applicable requirements according to the basis of order

Ordered with reference to steel names in the tablesRequirement
B.2, B.3, B.4 or B.5Chemical composition according to B.2; mechanical properties according to B.3, B.4 and B.5.
B.2, B.3, B.4, B.5, B.6 or B.7Chemical composition according to B.2; mechanical properties according to B.3, B.4 and B.5; hardenability values according to B.6 and B.7.

Supplementary or special requirements under Annex E apply if agreed at the time of enquiry and order.

Source: ISO 4954:2018, Table B.1, page 22. This table gives the standard relationship between product form, delivery condition and requirements; actual supply must be confirmed separately.

2. Chemical composition

Table B.2 – Chemical composition of case-hardening steels (cast analysis)

These are the standard’s reference requirements for cast analysis of C10E2C, not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

ElementMass fraction, %
C0.08–0.12
Si≤0.30
Mn0.30–0.60
P≤0.025
S≤0.025
Cr—
Ni—
Mo—
B—
Cu≤0.25

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials of elements that could impair hardenability, mechanical properties or suitability.

Al of 0.020–0.050% may be added to improve cold-heading performance.

a: Single values are maximum limits unless otherwise indicated. A dash does not mean zero content.

b: For steels with hardenability requirements under Tables B.6 and B.7, small departures from the specified limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 2 for the other elements.

c: A lower silicon content or a specified silicon range may be agreed at the time of order.

Source: ISO 4954:2018, Table B.2, page 23 (PDF page 29). The table and notes do not replace the complete standard.

3. Mechanical properties

Table B.3 – Mechanical properties of non-alloy steels

Steel nameDiameterDelivery condition
+AR or +PE+AC or +AC+PE+AR+C+AR+C+AC+AR+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZ min., % (a)Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
C10E2C25——————3906743065——
C10E2C510450584006554056380674206549062
C10E2C1040450584006553056380674206548062
C10E2C401004505840065————————

a: The Z values in condition +AR or +PE are given for information only.

Source: ISO 4954:2018, Table B.3, page 25. Rm is tensile strength; Z is reduction of area at fracture. HB denotes Brinell hardness where specified. The values apply only to the specified diameter intervals and delivery conditions.

4. Hardenability requirements

ISO 4954:2018, Tables B.6 and B.7, gives no hardenability values for this steel grade. Values from other steel grades have not been transferred.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — C10E2C

Basis: ISO 4954

Chemical composition source: ISO 4954:2018

Transcribed from the cited standard

Original source wording

Table B.2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.1300–0.2367

Missing elements: Cr, Mo, V, Ni

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.0950–0.1725

Missing elements: Cr, Ni, Mo, V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Known-element contribution, not a complete value: 0.1100–0.1925

Missing elements: Mo, Cr, Ni

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

WhatsApp Technical enquiry →
Image and content use · Creation Group