Composition source and applicability
Reference composition for the stated standard edition, not heat analysis. Confirm the order standard and the separate requirements for feedstock and finished product.
41CrNiMoS2 · ISO 4954:2018
| Element | Mass fraction / % |
|---|---|
| C | 0.37–0.44 |
| Si | ≤0.3 |
| Mn | 0.7–1 |
| P | ≤0.025 |
| S | 0.02–0.04 |
| Cr | 0.4–0.6 |
| Ni | 0.4–0.7 |
| Mo | 0.15–0.3 |
| Cu | ≤0.25 |
Source: ISO 4954:2018




1. Delivery conditions and applicable requirements
Table C.1 – Combinations of heat-treatment condition at delivery, product form and applicable requirements
| Delivery condition | Symbol | Wire rod | Bar | Wire |
|---|---|---|---|---|
| Hot rolled or peeled | +AR or +PE | X | X | X |
| Cold drawn | +AR+C | — | X | X |
| Cold drawn and spheroidize annealed | +AR+C+AC | — | X | X |
| Cold drawn, spheroidize annealed and lightly cold drawn | +AR+C+AC+LC | — | X | X |
| Spheroidize annealed or spheroidize annealed and peeled | +AC or +AC+PE | X | X | X |
| Spheroidize annealed and cold drawn | +AC+C | — | X | X |
| Spheroidize annealed, cold drawn and spheroidize annealed again | +AC+C+AC | — | X | X |
| Spheroidize annealed, cold drawn, spheroidize annealed again and lightly cold drawn | +AC+C+AC+LC | — | X | X |
X = applicable; — = not applicable.
Other delivery conditions may be agreed at the time of order.
Applicable requirements according to the basis of order
| Ordered with reference to steel names in the tables | Requirement |
|---|---|
| C.2, C.3, C.4, C.5 or C.6 | Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6. |
| C.2, C.3, C.4, C.5, C.6, C.7, C.8 or C.9 | Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; hardenability values according to C.7, C.8 and C.9. |
| C.2, C.3, C.4, C.5, C.6 or C.10 | Chemical composition according to C.2 and C.3; mechanical properties according to C.4, C.5 and C.6; minimum core hardness and maximum diameter according to C.10. |
Supplementary or special requirements under Annex E apply if agreed at the time of enquiry and order.
Source: ISO 4954:2018, Table C.1, page 34. This table gives the standard relationship between product form, delivery condition and requirements; actual supply must be confirmed separately.
2. Chemical composition
Table C.2 – Chemical composition of steels without boron for quenching and tempering (cast analysis)
These are the standard’s reference requirements for cast analysis of 41CrNiMoS2, not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.
Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials of elements that could impair hardenability, mechanical properties or suitability.
Al of 0.020–0.050% may be added to improve cold-heading performance.
a: Single values are maximum limits unless otherwise indicated. A dash does not mean zero content.
b: For steels with hardenability requirements under Tables C.7 and C.9, small departures from the specified limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 2 for the other elements.
c: A carbon range 0.04 percentage points wide, for example 0.33–0.37%, may be agreed at the time of enquiry and order.
d: A lower silicon content may be agreed at the time of order. Its effects on the specified properties, such as hardenability, must then be assessed.
Source: ISO 4954:2018, Table C.2, page 36 (PDF page 42). The table and notes do not replace the complete standard.
3. Mechanical properties
Table C.5 – Mechanical properties of alloy steels without boron
| Steel name | Diameter | Delivery condition | ||||||
|---|---|---|---|---|---|---|---|---|
| +AC or +AC+PE | +AC+C+AC | +AC+C+AC+LC | ||||||
| over, mm | up to and including, mm | Rm max., MPa | Z min., % | Rm max., MPa | Z min., % | Rm max., MPa | Z min., % | |
| 41CrNiMoS2 | 2 | 5 | — | — | 640 | 60 | 680 | 55 |
| 41CrNiMoS2 | 5 | 40 | — | — | 640 | 60 | 680 | 55 |
Source: ISO 4954:2018, Table C.5, page 40. Rm is tensile strength; Z is reduction of area at fracture. The values apply only to the specified diameter intervals and delivery conditions.
4. Hardenability requirements
Table C.7 – Hardness limits for steels without boron with specified normal hardenability (+H)
| Steel name | Symbol | Austenitizing temperature, °C (±5 °C) | Limit | Hardness, HRC, at distance from the quenched end, mm | |||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 1 | 2 | 3 | 4 | 5 | 6 | 7 | 8 | 9 | 10 | 11 | 13 | 15 | 20 | 25 | 30 | ||||
| 41CrNiMoS2 | +H | 850 | max. | 60 | 60 | 60 | 59 | 58 | 57 | 55 | 54 | 48 | 42 | 40 | 38 | 37 | 37 | 36 | — |
| 41CrNiMoS2 | +H | 850 | min. | 53 | 53 | 52 | 50 | 47 | 42 | 38 | 35 | 30 | 28 | 26 | 25 | 24 | 24 | 23 | — |
Source: ISO 4954:2018, Table C.7, page 45.
Table C.9 – Hardness limits for steels without boron with restricted hardenability bands (+HH and +HL)
| Steel name | Symbol | Austenitizing temperature, °C (±5 °C) | Limit | Hardness, HRC, at distance from the quenched end, mm | ||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 1.5 | 3 | 5 | 7 | 9 | 11 | 13 | 15 | 20 | 25 | 30 | 35 | 40 | 45 | 50 | ||||
| 41CrNiMoS2 | +HH | 850 | max. | 60 | 60 | 60 | 59 | 58 | 57 | 55 | 54 | 48 | 42 | 40 | 38 | 37 | 37 | 36 |
| 41CrNiMoS2 | +HH | 850 | min. | 55 | 55 | 55 | 53 | 51 | 47 | 44 | 41 | 36 | 33 | 31 | 29 | 28 | 28 | 27 |
| 41CrNiMoS2 | +HL | 850 | max. | 58 | 58 | 57 | 56 | 54 | 52 | 49 | 48 | 42 | 37 | 35 | 34 | 33 | 33 | 32 |
| 41CrNiMoS2 | +HL | 850 | min. | 53 | 53 | 52 | 50 | 47 | 42 | 38 | 35 | 30 | 28 | 26 | 25 | 24 | 24 | 23 |
a: This table does not apply to steels ordered with a restricted carbon range; see footnote c to Table C.2.
Source: ISO 4954:2018, Table C.9, page 49.
These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.