20NiCrMo2-2 Cold-drawn steel wire product image
20NiCrMo2-2 · Cold-drawn steel wire
01Applicable standardEN 10263-3:2017
02Material grade20NiCrMo2-2
03Product formCold-drawn steel wire
04Delivery informationTo be confirmed against the order technical requirements

Material technical data

Only data directly related to this material is shown here. Inspection, equipment, process and packaging information is linked separately.

Enquire this grade

1. Delivery conditions and applicable requirements

Table 1 – Delivery conditions, product forms and applicable requirements

Heat-treatment conditionSymbolWire rodBarWire
UntreatedNone or +UXXX
Spheroidize annealed+ACXXX
Treated to a ferrite-pearlite structure and specified hardness range+FP—X—
Basis of orderApplicable requirements
Table 3, 5 or 6 or 7Chemical composition according to Tables 3 and 4; mechanical properties according to Table 5, 6 or 7.
Table 3, 5 or 6 or 7, 8 or 9Chemical composition according to Tables 3 and 4; mechanical properties according to Table 5, 6 or 7; hardenability according to Table 8 or 9.
Table 3, 5, 6, 7, 8 or 9Supplementary or special requirements under Annex A of EN 10263-1:2017, if agreed at the time of enquiry and order.

Table 2 – Surface condition at delivery

Basis of agreementSurface conditionSymbolBarWire rodWire
Unless otherwise agreedAs rolledNone or +ARXX—
Special surface condition by agreementCold drawn+CX—X
Special surface condition by agreementLightly cold drawn+LCX—X
Special surface condition by agreementPeeled+PEXXX

X = applicable; — = not applicable. Other delivery conditions may be agreed at the time of order.

Heat-treatment condition and surface condition are separate requirements. This table gives the standard reference; the actual product form, delivery condition and suitability must be confirmed in the order.

Source: EN 10263-3:2017, Table 1 and 2, page 7–8 (PDF page 9–10).

2. Chemical composition

Table 3 – Chemical composition of case-hardening steels (cast analysis)

Reference requirements for 20NiCrMo2-2, steel number 1.6523. These are not analysis results for a particular heat. The order standard and requirements for raw material and finished product must be confirmed separately.

ElementMass fraction, %
C0.17–0.23
Si≤0.30
Mn0.65–0.95
P≤0.025
S≤0.025
Cr0.35–0.70
Mo0.15–0.25
Ni0.40–0.70
B—
Cu≤0.25

Values are mass fractions in percent. Single values are maximum limits unless otherwise indicated. “—” represents a blank source field and does not mean zero content.

Elements not listed must not be intentionally added without the purchaser’s agreement, except for finishing the heat. Appropriate precautions are required to prevent additions from scrap or other production materials that could impair hardenability, mechanical properties or suitability.

For steels with hardenability requirements under Tables 8 and 9, small departures from the composition limits are permitted, except for sulfur and phosphorus. Departures must not exceed 0.01% for carbon or the values in Table 4 for the other elements.

An aluminium addition of 0.020–0.050% is possible to improve cold-heading performance.

A lower silicon content or a specified silicon range may be agreed at the time of order.

Table 4 – Permissible deviations for product analysis

ElementLimiting values for cast analysis, %Permissible deviation for product analysis, %
C≤0.24±0.02
Si≤0.30±0.03
Mn≤1.00±0.04
Mn>1.00 and ≤1.40±0.06
P≤0.025+0.005
S≤0.040+0.005
Cr≤1.70±0.05
Mo≤0.30±0.03
Mo>0.30 and ≤0.50±0.04
Ni≤1.00±0.03
Ni>1.00 and ≤1.70±0.05
B≤0.0050±0.0003
Cu≤0.25+0.03

± means that, within one heat, the product analysis for an element may deviate above the upper limit or below the lower limit in Table 3, but not in both directions at the same time.

For steels with a specified sulfur range of 0.020–0.040% in the cast analysis, the permissible deviation is ±0.005%.

Source: EN 10263-3:2017, Table 3 on page 9 (PDF page 11), and Table 4 on page 10 (PDF page 12). These tables do not replace the complete standard.

3. Mechanical properties

Table 7 – Mechanical properties of alloy steels in the specified delivery condition

Steel nameSteel numberDiameterDelivery condition
+AC+FP+U+C+AC+U+C+AC+LC+AC+C
over, mmup to and including, mmRm max., MPaZ min., %HB min.HB max.Rm max., MPaZ min., %Rm max., MPaZ min., %Rm max., MPaZ min., %
20NiCrMo2-21.652325————5906263060——
20NiCrMo2-21.652351059060149194570626106072057
20NiCrMo2-21.6523104059060149194570626106071057

For +FP, the table specifies minimum and maximum Brinell hardness HB. These columns do not specify tensile strength or reduction of area.

Source: EN 10263-3:2017, Table 7, page 14. Rm is tensile strength; Z is reduction of area at fracture. The values apply to the specified diameter intervals and delivery conditions. A dash does not mean zero or confirm availability.

4. Hardenability requirements

Table 8 – Hardness limits for normal hardenability (+H)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.535791113152025303540
20NiCrMo2-21.6523+H920max.49484542363331302725242423
20NiCrMo2-21.6523+H920min.413731252220———————

Source: EN 10263-3:2017, Table 8, page 16.

Table 9 – Hardness limits for restricted hardenability bands (+HH and +HL)

Steel nameSteel numberSymbolAustenitizing temperature, °C (±5 °C)LimitHardness, HRC, at distance from the quenched end, mm
1.535791113152025303540
20NiCrMo2-21.6523+HH920max.49484542363331302725242423
20NiCrMo2-21.6523+HH920min.4441363127242221—————
20NiCrMo2-21.6523+HL920max.464440363129272623212020—
20NiCrMo2-21.6523+HL920min.413731252220———————

Source: EN 10263-3:2017, Table 9, page 18.

These values are standard references for the specified test conditions. They do not confirm availability, suitability for a particular cross-section or a production heat-treatment procedure. Delivery requirements require technical assessment.

Application and ordering note

Chemical composition, mechanical properties, delivery condition and other technical requirements are subject to the currently applicable standard edition, customer drawings and the order technical agreement. Website information does not replace formal quality certification documents.

What to include in the enquiry

Carbon equivalent calculator — 20NiCrMo2-2

Basis: EN 10263

Chemical composition source: EN 10263-3:2017 · Table 3

Transcribed from the cited standard

Composition is taken from the reviewed Table 3 above. The composition row was checked against DIN EN 10263-3:2018-02, the German version of EN 10263-3:2017. No boron limit is assigned to 20NiCrMo2-2. Unknown elements remain unknown. Confirm the applicable contract edition separately.

Original source wording

Table 3

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15Known-element contribution, not a complete value: 0.4050–0.6417

Missing elements: V

IIW/CEV: carbon and low-alloy steel weldability screening.

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5BKnown-element contribution, not a complete value: 0.2367–0.3633

Missing elements: V, B

Pcm: mainly low-carbon, low-alloy steels; confirm applicability, particularly when C exceeds 0.11%.

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40Calculated range: 0.2775–0.4150

CET: ferritic-steel preheat assessment; confirm EN 1011-2 conditions.

A stated upper limit means 0 to that limit. A lower limit alone does not define an upper bound. Missing elements are unknown, not zero. Standard-limit combinations are not measured heat results.

Carbon equivalent supports weldability assessment; it does not approve cold heading, fastener strength or a welding procedure. These formulas do not directly apply to stainless steels, cast irons or non-ferrous metals.

Method reference: TWI

Carbon equivalent calculator →

Send a technical enquiry

Contact technical team →

Material reference data

Same-grade reference does not establish standard equivalence, supply or substitution approval.

20NiCrMo2-2 · ISO 683-3:2022

Chemical composition · Cast analysis

Mass fraction %; Table 3, page 18 of the user's PDF. Unlisted elements must not be treated as 0; intentional addition of unlisted elements is subject to the standard and ordering agreement.

ElementMass fraction / %
C0.17~0.23
Si≤0.4
Mn0.65~0.95
P≤0.025
S≤0.035
Cr0.35~0.7
Mo0.15~0.25
Ni0.4~0.7
Cu≤0.4

When A.4 is expressly selected in the order, Si≥0.15% may be agreed; the basic table still specifies Si≤0.40%.

Delivery conditions and hardness · Table 7

Brinell hardness. +S: treated to improve shearability; +A: soft annealed; +TH: treated to a specified hardness range; +FP: treated to a ferrite-pearlite structure; +N: normalized. “—” means no requirement is specified for that delivery condition.

Delivery conditionBrinell hardness requirement
+S—
+A≤212
+TH161~212
+FP149~194
+N—

Heat treatment and test-piece conditions · Table 8

ItemTemperature / ℃
Austenitizing temperature for the end-quench test900 ± 5
Carburizing temperature (guidance)880~980
Direct and first quenching temperature (guidance)820~860
Second quenching: core quenching temperature (guidance)860~900
Second quenching: case quenching temperature (guidance)780~820
Tempering temperature (guidance)150~200

Except for the end-quench austenitizing temperature, carburizing, quenching and tempering temperatures are guidance values; the actual process must achieve the required properties. Guidance holding times are at least 30 minutes for austenitizing and at least 1 hour for tempering. Select the quenching medium according to product shape, cooling conditions and furnace load.

Hardenability conditions · Tables 5 and 6

Distance from the quenched end in mm; hardness in HRC. Apply only when the corresponding hardenability condition is specified in the order. “—” indicates that no limit is specified at that position.

+H · Normal hardenability
Limit / Distance mm1.535791113152025303540
Maximum49484542363331302725242423
Minimum413731252220———————
+HH · Restricted hardenability band
Limit / Distance mm1.535791113152025303540
Maximum49484542363331302725242423
Minimum4441363127242221—————
+HL · Restricted hardenability band
Limit / Distance mm1.535791113152025303540
Maximum464440363129272623212020—
Minimum413731252220———————
Permissible deviations in product analysis · Table 4
ElementSpecified cast-analysis range / %Permissible product-analysis deviation / %
C0.07<C≤0.31±0.02
Si≤0.40±0.03
Mn≤1.00 / >1.00~1.65±0.04 / ±0.06
P≤0.025+0.005
S≤0.040±0.005
Cr≤1.80±0.05
Mo≤0.30 / >0.30~0.50±0.03 / ±0.04
Ni≤1.00 / >1.00~2.00 / >2.00~3.50±0.03 / ±0.05 / ±0.07
Cu≤0.40+0.05
B≤0.0050±0.0003

“±” permits a deviation for a single cast above the upper limit or below the lower limit, in one direction only. Product-analysis deviations do not change the cast-analysis limits in Table 3.

Standard edition and ordering notes

The standard covers products including wire rod. Finished cold-heading wire supply, processing and properties require technical review and order confirmation. — means not specified in this table, not 0.

Source comparison: reviewed by Codex against the standard supplied by the user. This webpage does not replace the official standard, order agreement or inspection certificate.