← BackMaterial grade directory

1006

8 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 1006 →

1006 · SAE J 403-2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
SAE J403 NOV2001
Table / clause
Table 1 and Notes 1, 2 and *
PDF page references
1、3、4

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table 1, general applications, including wire rod; Mn .25–.40%
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Structural sections, plate, strip, sheet and welded tube; Mn≤.45%, with no minimum
IIW / CEV:0.0000–0.1550 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0000–0.1025Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0000–0.1250 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Table 1 UNS G10060 corresponds to SAE 1006, heat analysis wt%. ; Si is not a uniform mandatory component; When required, common ranges for bar products/semi-finished products are ≤ .10, .10–.20, .15–.35, .20–.40, .30–.60%; wire rod has a separate range of .07–.15%; No single range has been arbitrarily selected in this record. ; When Cu is required, it is generally specified as ≥.20%, which is not a uniform Cu upper limit or a default requirement. ; Addition of Pb .15–.35% requires L identification and a change to the UNS; Addition of B .0005–.003% requires B identification and shall not be merged into ordinary grades. ; Lower P/S for certain qualities/products must be verified separately per J411 and shall not apply agreement values from subsequent years. ; A requirement to report additional elements does not establish uniform limits for those elements in this table.; Unspecified Si/Cr/Ni/Mo etc. shall not be filled as zero; Finished product deviation to be verified separately per J409. ; Note * Mn≤.45% applies only to the aforementioned products and shall not be automatically applied to wire rod.

Original condition-branch records

Table 1, general applications, including wire rod; Mn .25–.40%

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Structural sections, plate, strip, sheet and welded tube; Mn≤.45%, with no minimum

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn≤ 0.45 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Official English Table 1 and footnotes visually checked.

1006 · ASTM A29/A29M-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ASTM A29/A29M-2012
Table / clause
Table 1, footnotes A–G
PDF page references
1、3、4

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1033 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0158–0.1067 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0175–0.1117 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0192–0.1133 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0225–0.1200 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0225Known-element contribution; incomplete value; missing Si, Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0225Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0258Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0275Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0292Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0325Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Original 2012 Table 1: ladle composition, mass fraction (wt%); applicability and deviations for product analysis must be checked separately under 4.3 and Table 5. Grade designations and product forms are retained as listed in the standard; cold-heading suitability is not implied. Note B: Si is an order-specific option; if not specified, it is unknown, not zero. Note C: Cu ≥0.20% applies only when ordered; no upper limit is invented, and ordinary orders do not automatically include Cu. Note D: Pb 0.15–0.35% applies only to an expressly designated leaded L grade; Pb is not added automatically to grades without L. Note F: additions of Bi/Ca/Se/Te are determined by agreement between purchaser and supplier; absent a specified value, they are not zero. Note E: boron treatment gives an expected content under specified conditions and is not a uniform B limit for all ordinary grades.

Original condition-branch records

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Order explicitly adopts Si ≤0.1% under note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2

Order explicitly adopts Si 0.15–0.35% under note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35

Order explicitly adopts Si 0.2–0.4% under note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4

Order explicitly adopts Si 0.3–0.6% under note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6
Cu≥ 0.2 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

The 2012 Table 1 and footnotes have been checked; order-specific optional compositions and base-table limits remain separate.

1006 · POSCO wire rod catalogue (local archive 1203; original edition not stated)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Local file 1203 (wire-rod pdf); the original does not state a publication edition; PDF metadata 2014-12-03 is only the file generation time
Document title
Wire rod
Table / clause
Printed page 14, composition table 3 (local table index)
PDF page references
8
Unit
Percentages as stated in the original table; refer to the source for the specific basis
Analysis type
The catalog does not consistently specify heat or product analysis
Manufacturer
POSCO

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.0417–0.1467Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

POSCO local wire rod catalogue, PDF page 8

printed page 14, table index 2, row 2. The original edition number is not stated; the PDF creation date 2014-12-03 is not the standard publication year. Manufacturer range information does not constitute our supply guarantee. Condition: the original table lists several alternative Si ranges; footnotes require confirmation by grade and between purchaser and supplier. Do not merge all options into one broad range or select any option by default.

Composition conditions

Verification notes

The original PDF tables and text coordinates were reconciled in both directions. Missing grade cells were restored; merged cells, footers and remarks were checked separately. Tables with identified disputes and rows without composition data are withheld.

1006 · Nippon Steel Wire Rods EXE203 2008.3 / SAE J403 NOV.2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Cat. No. EXE203 2008.3 PDF; cover copyright 2008
Document title
Nippon Steel Wire Rods
Table / clause
Printed page 10, table index 0
PDF page references
7
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
NIPPON STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.0417–0.1467Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Nippon Steel wire rod catalogue EXE203 (historical material, 2008.3), PDF p. 7

printed p. 10, SAE J403 NOV.2001. The source table does not specify the analysis type. Manufacturer-range data, not a standard-guaranteed value or heat-lot test, and not a representation of our supply. Condition: Si is an optional value subject to agreement as stated in the source; do not select by default or merge into one broad range. Until selected, do not use it in a complete calculation or assessment. Pb 0.15–0.35 and B 0.0005–0.0030 are optional additions with L/B designation; do not add them automatically to ordinary grades. Special low-P/S quality requires separate agreement verification.

Composition conditions

Verification notes

Grouped tables were expanded in full and checked against original images and notes. Ordinary, residual and conditional elements are kept separate; suffix tables lacking complete base-steel composition are excluded.

1006 · CHINA STEEL CORPORATION · Bars and Wire Rods Product Catalogue 2014-C1 / 7.1.15 SAE · Carbon steels (Edition unspecified)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Bars and wire rod
Original record status
Manufacturer source verified
Document edition
CAT.NO.3-BD-01-2014-C1 (stated on the back cover)
Document title
Bars and Wire Rods Product Catalogue
Table / clause
7.1.15 SAE · Carbon steels (Edition unspecified)
PDF page references
22
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
CHINA STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.0417–0.1467Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

China Steel bar and wire rod catalogue CAT.NO.3-BD-01-2014-C1, PDF p. 22

printed p. 20, §7.1.15 SAE carbon steels (edition not marked). The source table does not specify the analysis type. Historical manufacturer range data, not a standard-guaranteed value or heat-lot test, and not a representation of our supply. Conditions: Si is an agreement-based option, with separate options for bar and wire rod; B is not automatically added to the ordinary grades in the source table. Where Cu is specified, it is generally ≥0.20%; this is not a default Cu minimum for all steels.

Composition conditions

Verification notes

Merged cells in all 28 catalogue tables were reconstructed geometrically, with no missing cells. Original images, continuation pages and notes are recorded; disputed conditions are withheld.

1006 · SAE J403 (FHS catalogue; referenced year not stated)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Catalog edition not stated; archived original
Document title
FHS Wire Rod Product Manual (English edition)
PDF page references
6
Unit
wt.%
Analysis type
Analysis type not specified
Manufacturer
Formosa Ha Tinh Steel Corporation (FHS)

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Archived manufacturer FHS catalogue; edition and referenced-standard year are not stated; PDF page 6

printed page 5, 3.1.1. Chemical composition wt.%, analysis type not stated; not guaranteed standard limits or heat-specific measurements; Missing entries are not filled with 0.

Composition conditions

Verification notes

Original table cells and applicable footnotes checked; residual-element limits were not borrowed across clauses.

1006 · ASTM A29/A29M-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ASTM A29/A29M-2023
Table / clause
Table 1, footnotes A–G
PDF page references
4
Unit
Mass fraction (wt%)
Analysis type
Heat analysis (composition ranges and limits in the original table)

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under Table 1 note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1033 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under Table 1 note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0158–0.1067 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under Table 1 note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0175–0.1117 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under Table 1 note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0192–0.1133 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under Table 1 note B
IIW / CEV:0.0417–0.1467 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0225–0.1200 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0225Known-element contribution; incomplete value; missing Si, Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0225Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0258Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0275Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0292Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.0550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.0325Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.0350Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

ASTM A29/A29M-2023 original Table 1: base entries are ladle-analysis mass fraction wt%; product-analysis tolerances are checked separately under 4.3 and Table 5, not added to ladle limits. Orders by Table 1 grade must meet its ladle limits under 4.1.1; other ordered chemistries are separately agreed under 4.1.2 and Tables 3/4 and must not be mixed into this table. General hot-wrought bar requirements do not, by chemistry alone, establish cold-heading suitability, supply or mechanical properties. Note B: the Si range is a common option only when required by the order; Si is unspecified by default, not a universal range or zero. Note C: Cu≥0.20% applies only when expressly required by the order and has no added upper limit. Note D: leaded steel Pb is 0.15–0.35%; retain L as part of the grade identity, not ordinary grades. If lead is added to the ladle stream, its cast or ladle-analysis value cannot be determined. Note F: Bi/Ca/Se/Te are specified by buyer-supplier agreement; do not enter zero when no value is given. Note E: only for expressly specified boron treatment of killed steel, expected B is 0.0005–0.003%; where usual Ti addition is not permitted, up to 0.005% may be expected. These are not mandatory B limits for all ordinary grades.

Original condition-branch records

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Order explicitly adopts Si ≤0.1% under Table 1 note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)

Order explicitly adopts Si 0.1–0.2% under Table 1 note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2

Order explicitly adopts Si 0.15–0.35% under Table 1 note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35

Order explicitly adopts Si 0.2–0.4% under Table 1 note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4

Order explicitly adopts Si 0.3–0.6% under Table 1 note B

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si ≤0.1% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.1–0.2% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.15–0.35% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.2–0.4% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.3–0.6% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6
Cu≥ 0.2 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

Existing OCR of the four-page, 190-row original 2023 table was parsed cell by cell. All values were screened for differences against independent 2012 data and checked against the original 2023 images and footnotes; no values were filled from the older edition.

1006 · SAE J403-2014

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
SAE J403-2014
Table / clause
Table 1
PDF page references
3
Unit
Mass fraction (wt%)
Analysis type
Cast or heat analysis

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group B (default unless otherwise agreed)
IIW / CEV:0.0417–0.2387Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1357Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1598 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group A
IIW / CEV:0.0417–0.2153Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1248Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1485 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group C
IIW / CEV:0.0417–0.2840Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1497Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1770 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group D (no limit specified, but reporting is required)
IIW / CEV:0.0417–0.1467Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0125–0.1000Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0250–0.1200Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group B (default unless otherwise agreed)
IIW / CEV:0.0000–0.2470Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0000–0.1382Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0000–0.1648 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Flat products: sections, plate, strip, sheet and welded tube (as defined in Note 1); residual category A
IIW / CEV:0.0000–0.2237Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0000–0.1273Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0000–0.1535 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group C
IIW / CEV:0.0000–0.2923Known-element contribution; incomplete value; missing V; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0000–0.1522Known-element contribution; incomplete value; missing Si, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0000–0.1820 Independent-element envelope of standard ranges, not measured heat results; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group D (no limit specified, but reporting is required)
IIW / CEV:0.0000–0.1550Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0000–0.1025Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0000–0.1250Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≤ 0.35 (lower limit not stated)
Ni≤ 0.25 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Original SAE J403 Revised JUN2014 Table 1 cast or heat-analysis mass fractions wt%; Product-analysis tolerances are applied separately under SAE J409; J409 is not used to widen this table. UNS G10060 and SAE 1006 are names directly listed on the same row of this table; other standards or editions are not conflated with this edition. Where residual elements are not specified separately, the default is B; A/B/C is selected for the corresponding form or agreement; D has no tabulated limit, but the quantity of Cu/Ni/Cr/Mo must still be reported and is not treated as zero. To demonstrate compliance with the table, Cu/Cr/Ni/Mo/Si must be reported in addition to C/Mn/P/S; Below 0.02%, the original document permits reporting as <0.02%; this is neither a universal maximum nor zero. P/S conditions for flat and long products must be selected separately; the wider maxima must not be combined; 1006/1008 Mn is selected by form under Table 1, note 6/7. Si is specified only by agreement in the order; Common wire-rod options are ≤0.10, 0.07–0.15, 0.10–0.20, 0.15–0.35, 0.20–0.40 and 0.30–0.60%; The common 0.07–0.15 option is not listed for other products. Contract values must be checked against product form; no fixed Si is entered without agreement. Ordinary grades in this table do not automatically include Pb or B. Separately leaded or boron-treated grades require the L/B designation and the corresponding UNS; the original Pb0.15–0.35% and B0.0005–0.003% apply to that treatment condition and are not included in ordinary steel. Table 1, note 3: where Cu is specifically required, Cu≥0.20% is usually specified; The residual options in this batch control residual content only; intentional Cu addition conditions are not unconditionally combined with residual maxima. The specific ordering range requires separate agreement; this special Cu condition is not assessed automatically. Table 1, note 5: this row may be supplied as extra-low-carbon, IF-stabilized or unstabilized steel; Specific stabilizing elements and delivery conditions require separate verification; alloy limits not listed in this table are not invented. 3.1 and Table 6 require reporting of C/Mn/P/S/Si/Al/Cu/Ni/Cr/Mo/Nb(Cb)/Ti/V/B/N; As/Sb is additionally reported when requested by the purchaser. Si/Cu/Ni/Cr/Mo below 0.02% may be reported as <0.02%; Nb/Ti/V below 0.008% may be reported as <0.008%. These are reporting thresholds, not general composition maxima; they are not used to insert zeros or invent limits.

Original condition-branch records

Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group B (default unless otherwise agreed)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≤ 0.35 (lower limit not stated)
Ni≤ 0.25 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group A

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.15 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≤ 0.4 (lower limit not stated)
Ni≤ 0.4 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Mo≤ 0.12 (lower limit not stated)

Long products: forged semifinished products, hot-rolled/cold-finished bars, wire rod and seamless tubes; residual-element group D (no limit specified, but reporting is required)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn0.25 ~ 0.4
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group B (default unless otherwise agreed)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn≤ 0.45 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.35 (lower limit not stated)
Ni≤ 0.25 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Flat products: sections, plate, strip, sheet and welded tube (as defined in Note 1); residual category A

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn≤ 0.45 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.15 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group C

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn≤ 0.45 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.4 (lower limit not stated)
Ni≤ 0.4 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Mo≤ 0.12 (lower limit not stated)

Flat products: structural shapes, plate, strip, sheet and welded pipe (as defined in note 1); residual-element group D (no limit specified, but reporting is required)

ElementComposition requirement
C≤ 0.08 (lower limit not stated)
Mn≤ 0.45 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The original 2014 text was checked across four tables and 79 rows, including composition cells, product-form columns, UNS designations and notes; sources and distinct order conditions are retained separately.