← BackMaterial grade directory

X2CRNI18-9

17 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for X2CRNI18-9 →

Material demand assessment

Looking for X2CRNI18-9 material?

Not listed in our catalog? You are welcome to submit your requirements. We assess whether our equipment, production lines and process capabilities suit your grade, product form, dimensions, processing and delivery requirements, then discuss possible processing, trials or supply arrangements.

Feasibility and supply terms are confirmed after technical review. The standard information on this page is not a supply or performance commitment.

Explore products and processing capabilities

X2CrNi18-9 · EN 10263-5-2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Stainless steel
Subcategory
Austenitic stainless steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10263-5-2001
Table / clause
Table 2 and notes a–e; Table 3 is cited only for deviations
PDF page references
1、8、9

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Applicability and limitations

Actual source: DIN EN 10263-5:2002-02; German adoption of EN 10263-5:2001, PDF p. 8 Table 2 and Notes a–e.

Default is ladle analysis, mass fraction wt%; product-analysis deviations are separately governed by Table 3 and are not added to default ladle ranges.

Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); residual elements must not impair performance or use.

This older edition does not use the 2017 edition’s conditional sulfur provisions; do not copy newer machining/welding/polishing options.

For Ti-stabilized grades, verify 5×C≤Ti≤0.70% using measured C; do not apply this condition to grades without Ti.

The standard covers cold heading/cold extrusion; actual supply, dimensions, delivery condition and properties still require confirmation.

Original condition-branch records

Default heat-analysis values in historical Table 2

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Verification notes

Visual check of the previous-edition cover, all 19 grades in Table 2, and footnotes

X2CrNi18-9 · ISO 4954

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Stainless steel
Subcategory
Stainless steel
Material form
Cold-heading wire
Original record status
Source edition identified; composition verification pending
Standard edition
ISO 4954:2018
Table / clause
Table D.2

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.1 (lower limit not stated)
Cu≤ 1 (lower limit not stated)

Applicability and limitations

Composition based on ISO 4954:2018; the product edition is unspecified, so confirm the edition applicable to the contract.

Composition conditions

Verification notes

Composition based on ISO 4954:2018; the product edition is unspecified, so confirm the edition applicable to the contract.View associated products →

X2CrNi18-9 · ISO 4954-2018

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Stainless steel
Subcategory
Stainless steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ISO 4954:2018
Table / clause
Table D.2

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.1 (lower limit not stated)
Cu≤ 1 (lower limit not stated)

Applicability and limitations

ISO 4954:2018 Table D.2 gives cast analysis; single values are maxima and dashes are not zero.

Product-analysis deviations are listed separately under Tables 2/3, not used directly to relax cast-composition limits.

Elements not listed must not be intentionally added without the purchaser's consent, except for finishing the heat.

Verification notes

The original standard, Table D.2 and footnotes have been checked

X2CrNi18-9 · EN 10263-5-2017

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10263-5-2017
Table / clause
Table 3 and footnotes a–e

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default composition in Table 3
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Machinability condition S 0.015–0.030%
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Weldability condition S 0.008–0.030%
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Polishability recommendation S≤0.015%
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
N≤ 0.1 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Applicability and limitations

Heat-analysis mass fractions wt%; Product-analysis tolerances follow Table 4 separately. ; The sulfur conditions for machining, welding and polishing in Table 3, note b are retained separately; different requirements are not imposed simultaneously. ; Ti-stabilized grades require 5×C≤Ti≤0.70%, checked jointly with measured C/Ti. ; This standard covers stainless steel for cold heading and cold extrusion; delivery condition, dimensions, surface and mechanical properties still require independent confirmation. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; unspecified contents are not treated as zero.

Original condition-branch records

Default composition in Table 3

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
N≤ 0.1 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Machinability condition S 0.015–0.030%

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
N≤ 0.1 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Weldability condition S 0.008–0.030%

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
N≤ 0.1 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Polishability recommendation S≤0.015%

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
N≤ 0.1 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The original English Table 3 and footnotes have been checked

X2CrNi18-9 · EN 10269-2013

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10269-2013
Table / clause
Table 1 and notes a–c

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default sulfur content in Table 1
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
S 0.015–0.030% agreed at enquiry or ordering to improve machinability
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Weldability condition S 0.008–0.030% agreed at enquiry or ordering
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.1 (lower limit not stated)

Applicability and limitations

Heat-analysis mass fractions wt%; Product-analysis tolerances require separate verification under Table 2. ; The agreed sulfur condition in Table 1, note b applies only to grades marked b; default, machining and welding ranges are retained separately. ; This standard covers steels and nickel alloys for high- and low-temperature fasteners; cold-heading suitability is not established for every grade or delivery condition. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; Unspecified values are not treated as zero.

Original condition-branch records

Default sulfur content in Table 1

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.1 (lower limit not stated)

S 0.015–0.030% agreed at enquiry or ordering to improve machinability

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.1 (lower limit not stated)

Weldability condition S 0.008–0.030% agreed at enquiry or ordering

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.1 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The original English Table 1 and footnotes were checked

X2CrNi18-9 · DIN EN 10263-5-2002

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10263-5-2002
Table / clause
Table 2 and notes a–e; Table 3 is cited only for deviations
PDF page references
1、8、9

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Applicability and limitations

The original webpage states DIN EN 10263-5-2018; The composition in this record was actually verified against DIN EN 10263-5-2002; the edition is now identified as 2002 according to the original evidence; See the separate complete-table record for edition 2018. ; Source actually used: DIN EN10263-5:2002-02, the German-language adoption of EN10263-5:2001; PDF8, Table 2 and notes a–e. ; Default heat analysis in wt%.; Apply product-analysis tolerances in Table 3 separately; do not add them to the default heat-analysis range. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; Residual elements must not impair the properties or intended use. ; The older table does not use the 2017 edition’s separate sulfur conditions; do not copy machining/welding/polishing options from the newer edition.. ; For Ti-stabilized grades, check 5×C≤Ti≤0.70% against measured C.; Does not apply to grades for which Ti is not specified. ; Standard range for cold-heading and cold-extrusion; actual supply, dimensions, delivery condition, and performance still require confirmation..

Original condition-branch records

Default heat-analysis values in historical Table 2

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Verification notes

The original webpage states DIN EN 10263-5-2018; The composition in this record was actually verified against DIN EN 10263-5-2002; the edition is now identified as 2002 according to the original evidence; See the separate complete-table record for edition 2018.

X2CrNi18-9 · NF EN 10269-1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
NF EN 10269-1999
Table / clause
Table 1 · Notes 1/2
PDF page references
23

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table 1 default S≤.030%
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Recommended S .015–.030% to improve machinability
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

Applicability and limitations

Original text NF EN10269 cover novembre1999, Table 1 heat analysis mass fraction %. ; Table 1, Note 2: Sulfur .015–.030% is a recommended range for improved machinability; it does not replace the default maximum.; This note does not apply to 42CrMo4 as it is not marked. ; Elements not listed shall not be intentionally added without the purchaser's consent (except additions needed to finish steelmaking); blanks are not zero. ; Standards for high- and low-temperature fastener steels and nickel alloys; Composition alone does not prove that cold-heading wire is available or suitable for forming. ; Product-analysis deviations require separate verification under Table 2; they do not expand the default heat-analysis range.; Sulfur limits of the 2013 version do not apply.

Original condition-branch records

Table 1 default S≤.030%

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

Recommended S .015–.030% to improve machinability

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Values and notes in original NF, Table 1 were visually checked

X2CrNi18-9 · EN 10269-2006

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Historical-edition reference
Standard edition
NF EN 10269-1999
Table / clause
Table 1 · Notes 1/2
PDF page references
23

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table 1 default S≤.030%
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Recommended S .015–.030% to improve machinability
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

Applicability and limitations

The chemical composition currently shown is transcribed from the original NF EN 10269-1999; The original record cites EN 10269-2006; that original edition remains unavailable, and differences between editions have not been confirmed. Original text NF EN10269 cover novembre1999, Table 1 heat analysis mass fraction %. ; Table 1, Note 2: Sulfur .015–.030% is a recommended range for improved machinability; it does not replace the default maximum.; This note does not apply to 42CrMo4 as it is not marked. ; Elements not listed shall not be intentionally added without the purchaser's consent (except additions needed to finish steelmaking); blanks are not zero. ; Standards for high- and low-temperature fastener steels and nickel alloys; Composition alone does not prove that cold-heading wire is available or suitable for forming. ; Product-analysis deviations require separate verification under Table 2; they do not expand the default heat-analysis range.; Sulfur limits of the 2013 version do not apply.

Original condition-branch records

Table 1 default S≤.030%

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

Recommended S .015–.030% to improve machinability

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1 (lower limit not stated)
Mn≤ 2 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
Cr17.5 ~ 19.5
Ni8 ~ 10
N≤ 0.11 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The chemical composition currently shown is transcribed from the original NF EN 10269-1999; The original record cites EN 10269-2006; that original edition remains unavailable, and differences between editions have not been confirmed.

X2CrNi18-9 · DIN EN 10263-5-2002

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10263-5-2002
Table / clause
Table 2 and notes a–e; Table 3 is cited only for deviations
PDF page references
1、8、9

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Applicability and limitations

Actual source: DIN EN 10263-5:2002-02; German adoption of EN 10263-5:2001, PDF p. 8 Table 2 and Notes a–e. / Default is ladle analysis, mass fraction wt%; product-analysis deviations are separately governed by Table 3 and are not added to default ladle ranges. / Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); residual elements must not impair performance or use. / This older edition does not use the 2017 edition’s conditional sulfur provisions; do not copy newer machining/welding/polishing options. / For Ti-stabilized grades, verify 5×C≤Ti≤0.70% using measured C; do not apply this condition to grades without Ti. / The standard covers cold heading/cold extrusion; actual supply, dimensions, delivery condition and properties still require confirmation.

Composition conditions

Original condition-branch records

Default heat-analysis values in historical Table 2

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Verification notes

Visual check of the previous-edition cover, all 19 grades in Table 2, and footnotes

X2CrNi18-9 · DIN EN 10263-5-2002

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10263-5-2002
Table / clause
Table 2 and notes a–e; Table 3 is cited only for deviations
PDF page references
1、8、9

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Applicability and limitations

Actual source: DIN EN 10263-5:2002-02; German adoption of EN 10263-5:2001, PDF p. 8 Table 2 and Notes a–e. / Default is ladle analysis, mass fraction wt%; product-analysis deviations are separately governed by Table 3 and are not added to default ladle ranges. / Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); residual elements must not impair performance or use. / This older edition does not use the 2017 edition’s conditional sulfur provisions; do not copy newer machining/welding/polishing options. / For Ti-stabilized grades, verify 5×C≤Ti≤0.70% using measured C; do not apply this condition to grades without Ti. / The standard covers cold heading/cold extrusion; actual supply, dimensions, delivery condition and properties still require confirmation.

Composition conditions

Original condition-branch records

Default heat-analysis values in historical Table 2

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)
Cu≤ 1.0 (lower limit not stated)

Verification notes

Visual check of the previous-edition cover, all 19 grades in Table 2, and footnotes

X2CrNi18-9 · EN 10088-1-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10088-1-2005
Table / clause
Table 4 and continuation; notes a–e; all 50 austenitic corrosion-resistant steel grades
PDF page references
1、3、11、12

Source document

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Applicability and limitations

EN 10088-1:2005 Table 4 and continuation: ladle analysis (wt%); the official SIST adoption preview PDF, pages 11/12, covers all 50 grades and notes. Note a: unlisted elements are not intentionally added without purchaser consent, except as needed to complete steelmaking; a blank is not zero. Note b: for grades marked b only, S is selected separately for long products and by property requirement. Note d: the increased Ni maximum for special reasons applies only to listed grades, not all grades. Note c: Cu up to 1.0% for cold heading/extrusion; this condition path is provided here only for grades with blank Cu in the original table. Existing Cu alloy ranges retain their original values; the exception has not automatically rewritten them. The linked Ti≥5C/Nb≥10C and Ti≥8(C+N) conditions are retained; an unlisted N maximum is not zero. Note e: the source warns of skin-contact regulatory issues for high-sulfur free-machining steel; this is retained as a historical warning only and is not a claim of current compliance based on the 2005 text. Listed chemistry and the cold-heading Cu exception alone do not establish overall cold-heading performance or company supply; mechanical and product standards must be checked separately, and national adoption does not mean automatic equivalence.

Original condition-branch records

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Official source Table 4, all 50 rows and footnotes visually checked; conditional route for Cu cells left blank in the original.

X2CrNi18-9 · EN 10088-1-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10088-1-2005
Table / clause
Table 4 and continuation; notes a–e; all 50 austenitic corrosion-resistant steel grades
PDF page references
1、3、11、12

Source document

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Applicability and limitations

EN 10088-1:2005 Table 4 and continuation: ladle analysis (wt%); the official SIST adoption preview PDF, pages 11/12, covers all 50 grades and notes. Note a: unlisted elements are not intentionally added without purchaser consent, except as needed to complete steelmaking; a blank is not zero. Note b: for grades marked b only, S is selected separately for long products and by property requirement. Note d: the increased Ni maximum for special reasons applies only to listed grades, not all grades. Note c: Cu up to 1.0% for cold heading/extrusion; this condition path is provided here only for grades with blank Cu in the original table. Existing Cu alloy ranges retain their original values; the exception has not automatically rewritten them. The linked Ti≥5C/Nb≥10C and Ti≥8(C+N) conditions are retained; an unlisted N maximum is not zero. Note e: the source warns of skin-contact regulatory issues for high-sulfur free-machining steel; this is retained as a historical warning only and is not a claim of current compliance based on the 2005 text. Listed chemistry and the cold-heading Cu exception alone do not establish overall cold-heading performance or company supply; mechanical and product standards must be checked separately, and national adoption does not mean automatic equivalence.

Original condition-branch records

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Official source Table 4, all 50 rows and footnotes visually checked; conditional route for Cu cells left blank in the original.

X2CrNi18-9 · NF EN 10088-1-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Composition basis in the adopted standard verified
Standard edition
EN 10088-1-2005
Table / clause
Table 4 and continuation; notes a–e; all 50 austenitic corrosion-resistant steel grades
PDF page references
1、3、11、12

Source document

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category
Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.
IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Applicability and limitations

NF EN 10088-1:2005 adopts EN 10088-1:2005 (EN 10088-1-2005); See the data basis for the actual composition source file and table number. EN10088-1:2005 Table 4 and its continuation; heat analysis wt%; all 50 grades and footnotes on PDF pages 11/12 of the official SIST adoption preview.. ; Note a: Elements not listed shall not be intentionally added without the consent of the purchaser (except additions needed to finish steelmaking).; Blanks are not entered as zero. ; Note b: For grades marked b, S shall be selected separately according to long products and properties.; The increased Ni upper limit based on special reasons in Note d applies only to the listed steel grades and cannot be generalized to all grades.. ; Note c: For cold-heading/cold-extrusion applications, Cu max 1.0%.; This conditional path is provided only for grades where Cu was blank in the original table; existing Cu alloying ranges shall retain their original values, and their Cu exceptions have not been automatically rewritten.. ; The linkages Ti≥5C/Nb≥10C and Ti≥8(C+N) are retained.; If no N upper limit is listed, do not fill as zero.. ; Note e retains the original historical caution about skin-contact regulations for high-sulfur free-cutting steel; the 2005 text is not used to claim present-day compliance.. ; The listed compositions and the cold-heading Cu exception do not independently prove the overall cold-heading properties of the material or company supply.; Mechanical properties and product standards require separate verification; national adoption does not automatically establish equivalence..

Original condition-branch records

Default sulfur requirement; default Ni; the cold-heading Cu exception is not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Default sulphur requirement; default Ni; note c: Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, S for long products/wire etc.: ≤0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, S for long products/wire etc.: ≤0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for machining: 0.015–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for machining: 0.015–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.015 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for welding: 0.008–0.030%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for welding: 0.008–0.030%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S0.008 ~ 0.03
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

Note b, recommended S for polishing: ≤0.015%Default Ni; cold-heading Cu exception not selected, so the original-table Cu requirement applies.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5

Note b, recommended S for polishing: ≤0.015%Default Ni; note c allows Cu≤1.0% for cold heading/cold extrusion.

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
N≤ 0.11 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.5
Cu≤ 1.0 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The formal adoption relationship and corresponding EN composition original have been checked; the complete national adoption text has not been verified page by page.

X2CrNi18-9 · NF EN 10269:1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Stainless steel
Subcategory
Stainless steel
Material form
Reference record
Original record status
Original-standard record
Standard edition
NF EN 10269:1999
Table / clause
EN 10269:1999 Table 1 and footnotes 1 and 2
PDF page references
2、23

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
C≤ 0.03 (lower limit not stated)
Si≤ 1.0 (lower limit not stated)
Mn≤ 2.0 (lower limit not stated)
P≤ 0.045 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr17.5 ~ 19.5
Ni8.0 ~ 10.0
N≤ 0.11 (lower limit not stated)

Applicability and limitations

The cover of NF EN 10269:1999 explicitly adopts EN 10269:1999; Preserve the correspondence between the French adoption version and the European version; do not label as other countries or new editions. ; Table 1 gives heat-analysis mass percentages; Single values in P and S columns are upper limits; other single values are parsed according to the inequality signs in the original table; Unspecified elements shall not be filled as zero. ; Applies to billets, bars and wire rod of steels and nickel alloys for fasteners with specified high- or low-temperature properties.; Cold heading and actual supply must be verified in conjunction with delivery condition, dimensions, and process. ; Table 1 Footnote 1: Elements not listed in the table shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking); Elements that affect properties must be prevented from being introduced via scrap steel, etc.. ; This record only verifies the heat analysis composition in Table 1; product analysis tolerances in Table 2 shall not be automatically added to the heat limits. ; Footnote 2 of Table 1 only suggests controlling S within 0.015–0.030% to improve machinability; The suggested value shall not be treated as a mandatory S lower limit; the default remains S≤0.030%.

Combined limits

Combined-element limits

    X2CrNi18-9 · ISO 15510-2014

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material category
    Stainless steel
    Subcategory
    Stainless steel
    Material form
    Reference record
    Original record status
    Original standard verified
    Standard edition
    ISO 15510-2014
    Table / clause
    The current grade row in Table1; Note a and corresponding footnotes (original text on the publishing platform)
    PDF page references
    7

    Source document

    Carbon-equivalent reference

    Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

    Base range in Table 1
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category
    Note c: only where ferrite content must be reduced for a special reason, the Ni maximum may be increased by 0.50 percentage points; This condition must be confirmed
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category

    Composition record (conditional branches apply; this is not an unconditional requirement)

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)

    Applicability and limitations

    ISO 15510:2014, Table 1 gives heat analysis, mass fractions wt%; Under note a, values without a stated range or minimum are maxima; a dash is not treated as zero. Composition rows follow an excerpt of the official PDF edition; relevant footnotes follow the original Table 1 in the Sample text section of the standards publishing platform; Verification of the complete standard text or mechanical properties is not claimed. The standard covers material for wrought products, including ingots and semi-finished products; Similar composition does not establish direct substitution; cold-heading suitability and supply condition require separate confirmation. The S 0.015–0.030% machinability recommendations, 0.008–0.020% weldability recommendation and S≤0.015% polishability recommendation in note b concern specific properties and do not directly replace this row’s sulfur limits. Note c applies only where ferrite content must be reduced for special reasons such as hot workability or low magnetic permeability; The increased Ni maximum is not treated as an unconditional range.

    Original condition-branch records

    Base range in Table 1

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)

    Note c: only where ferrite content must be reduced for a special reason, the Ni maximum may be increased by 0.50 percentage points; This condition must be confirmed

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 11.0
    N≤ 0.1 (lower limit not stated)

    A condition branch must be selected

    Yes

    Verification notes

    The row for this grade in Table 1 has been checked against the official PDF; Relevant original footnotes are retained in the supporting verification record; Full standard text and mechanical properties to be verified separately

    X2CrNi18-9 · DIN EN 10263-5-2018

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material form
    Reference record
    Original record status
    Original standard verified
    Standard edition
    DIN EN 10263-5:2018-02
    Table / clause
    Tabelle 3 and footnote a–e; Tabelle 4 product-analysis tolerances require separate verification
    PDF page references
    1、10、11
    Unit
    Mass fraction (wt%)
    Analysis type
    Heat analysis

    Carbon-equivalent reference

    Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

    Default composition in Table 3
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category
    Machinability condition S 0.015–0.030%
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category
    Weldability condition S 0.008–0.030%
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category
    Polishability recommendation S≤0.015%
    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category

    Composition record (conditional branches apply; this is not an unconditional requirement)

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)
    Cu≤ 1.0 (lower limit not stated)

    Applicability and limitations

    DIN EN 10263-5:2018-02 is the German-language edition of EN 10263-5:2017; This record was verified against heat analysis and footnotes in Table 3 of the official German edition. ; Heat-analysis mass fractions wt%; Product-analysis tolerances follow Table 4 separately. ; The sulfur conditions for machining, welding and polishing in Table 3, note b are retained separately; different requirements are not imposed simultaneously. ; Ti-stabilized grades require 5×C≤Ti≤0.70%, checked jointly with measured C/Ti. ; This standard covers stainless steel for cold heading and cold extrusion; delivery condition, dimensions, surface and mechanical properties still require independent confirmation. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; unspecified contents are not treated as zero.

    Original condition-branch records

    Default composition in Table 3

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)
    Cu≤ 1.0 (lower limit not stated)

    Machinability condition S 0.015–0.030%

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S0.015 ~ 0.03
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)
    Cu≤ 1.0 (lower limit not stated)

    Weldability condition S 0.008–0.030%

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S0.008 ~ 0.03
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)
    Cu≤ 1.0 (lower limit not stated)

    Polishability recommendation S≤0.015%

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Si≤ 1.0 (lower limit not stated)
    Mn≤ 2.0 (lower limit not stated)
    P≤ 0.045 (lower limit not stated)
    S≤ 0.015 (lower limit not stated)
    Cr17.5 ~ 19.5
    Ni8.0 ~ 10.5
    N≤ 0.1 (lower limit not stated)
    Cu≤ 1.0 (lower limit not stated)

    A condition branch must be selected

    Yes

    Verification notes

    DIN EN 10263-5:2018-02 official German edition, Table 3, row 2 and notes a–e checked; adopts EN 10263-5:2017.

    X2CrNi18-9 · EN 10263

    Original-source verification is incomplete; this is not a formal standard reference

    Material category
    Stainless steel
    Subcategory
    Stainless steel
    Material form
    Drawn wire
    Verification status
    Published on the website; original-source verification pending

    Carbon-equivalent reference

    IIW / CEV: not directly applicable to this material category
    Pcm (Ito–Bessyo): not directly applicable to this material category
    CET: not directly applicable to this material category

    Composition

    ElementComposition requirement
    C≤ 0.03 (lower limit not stated)
    Cr17.5 ~ 19.5
    Cu≤ 1 (lower limit not stated)
    Mn≤ 2 (lower limit not stated)
    N≤ 0.11 (lower limit not stated)
    Ni8 ~ 10
    P≤ 0.045 (lower limit not stated)
    S≤ 0.03 (lower limit not stated)
    Si≤ 1 (lower limit not stated)

    Applicability and limitations

    Give priority to the published technical page on the Creation Group website. Use local reference ranges only as supplementary composition cross-checks; the applicable standard for that product page, the technical agreement and actual verification take precedence.