← BackMaterial grade directory

1030

17 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 1030 →

1030 · ASTM A29/A29M-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ASTM A29/A29M-2012
Table / clause
Table 1, footnotes A–G
PDF page references
1、3、4

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3883 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3133–0.3917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.3967 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3167–0.3983 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3200–0.4050 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Si, Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3233Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3250Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3267Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3300Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Original 2012 Table 1: ladle composition, mass fraction (wt%); applicability and deviations for product analysis must be checked separately under 4.3 and Table 5. Grade designations and product forms are retained as listed in the standard; cold-heading suitability is not implied. Note B: Si is an order-specific option; if not specified, it is unknown, not zero. Note C: Cu ≥0.20% applies only when ordered; no upper limit is invented, and ordinary orders do not automatically include Cu. Note D: Pb 0.15–0.35% applies only to an expressly designated leaded L grade; Pb is not added automatically to grades without L. Note F: additions of Bi/Ca/Se/Te are determined by agreement between purchaser and supplier; absent a specified value, they are not zero. Note E: boron treatment gives an expected content under specified conditions and is not a uniform B limit for all ordinary grades.

Original condition-branch records

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Order explicitly adopts Si ≤0.1% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2

Order explicitly adopts Si 0.15–0.35% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35

Order explicitly adopts Si 0.2–0.4% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4

Order explicitly adopts Si 0.3–0.6% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6
Cu≥ 0.2 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

The 2012 Table 1 and footnotes have been checked; order-specific optional compositions and base-table limits remain separate.

1030 · SAE J 403-2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
SAE J403 NOV2001
Table / clause
Table 1 and Notes 1, 2 and *
PDF page references
1、3、4

Carbon-equivalent reference

IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Table 1: UNS G10300 corresponds to SAE 1030; heat analysis, wt%. Si is not a universally mandatory constituent. When specified, common limits for bars/semi-finished products are ≤.10, .10–.20, .15–.35, .20–.40 and .30–.60%; wire rod also has the .07–.15% option. This record does not select a range without agreement. When Cu is required, ≥.20% is generally specified; this is neither a universal upper limit for Cu nor a default requirement. Addition of Pb at .15–.35% requires the L designation and a change to UNS; addition of B at .0005–.003% requires the B designation. These treatments are not included in ordinary grades. Lower P/S limits for certain qualities/products require separate verification against J411; agreement values from later editions are not imported. A requirement to report additional elements does not establish universal limits in this table. Unspecified Si/Cr/Ni/Mo and other elements are not assigned zero. Product-analysis deviations under J409 require separate verification.

Verification notes

Official English Table 1 and footnotes visually checked.

1030 · ASTM A29/A29M-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ASTM A29/A29M-2012
Table / clause
Table 1, footnotes A–G
PDF page references
1、3、4

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3883 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3133–0.3917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.3967 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3167–0.3983 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3200–0.4050 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Si, Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3233Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3250Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3267Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3300Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Original 2012 Table 1: ladle composition, mass fraction (wt%); applicability and deviations for product analysis must be checked separately under 4.3 and Table 5. Grade designations and product forms are retained as listed in the standard; cold-heading suitability is not implied. Note B: Si is an order-specific option; if not specified, it is unknown, not zero. Note C: Cu ≥0.20% applies only when ordered; no upper limit is invented, and ordinary orders do not automatically include Cu. Note D: Pb 0.15–0.35% applies only to an expressly designated leaded L grade; Pb is not added automatically to grades without L. Note F: additions of Bi/Ca/Se/Te are determined by agreement between purchaser and supplier; absent a specified value, they are not zero. Note E: boron treatment gives an expected content under specified conditions and is not a uniform B limit for all ordinary grades.

Original condition-branch records

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Order explicitly adopts Si ≤0.1% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2

Order explicitly adopts Si 0.15–0.35% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35

Order explicitly adopts Si 0.2–0.4% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4

Order explicitly adopts Si 0.3–0.6% under note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si ≤0.1% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.1–0.2% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.15–0.35% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.2–0.4% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.3–0.6% under note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6
Cu≥ 0.2 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

The 2012 Table 1 and footnotes have been checked; order-specific optional compositions and base-table limits remain separate.

1030 · POSCO wire rod catalogue (local archive 1203; original edition not stated)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Local file 1203 (wire-rod pdf); the original does not state a publication edition; PDF metadata 2014-12-03 is only the file generation time
Document title
Wire rod
Table / clause
Printed page 16, composition table 1 (local table index)
PDF page references
9
Unit
Percentages as stated in the original table; refer to the source for the specific basis
Analysis type
The catalog does not consistently specify heat or product analysis
Manufacturer
POSCO

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.3800–0.4900Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

POSCO local wire rod catalogue, PDF page 9

printed page 16, table index 0, row 2. The original edition number is not stated; the PDF creation date 2014-12-03 is not the standard publication year. Manufacturer range information does not constitute our supply guarantee. Condition: the original table lists several alternative Si ranges; footnotes require confirmation by grade and between purchaser and supplier. Do not merge all options into one broad range or select any option by default.

Composition conditions

Verification notes

The original PDF tables and text coordinates were reconciled in both directions. Missing grade cells were restored; merged cells, footers and remarks were checked separately. Tables with identified disputes and rows without composition data are withheld.

1030 · Nippon Steel Wire Rods EXE203 2008.3 / SAE J403 NOV.2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Cat. No. EXE203 2008.3 PDF; cover copyright 2008
Document title
Nippon Steel Wire Rods
Table / clause
Printed page 10, table index 0
PDF page references
7
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
NIPPON STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.3800–0.4900Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

Nippon Steel wire rod catalogue EXE203 (historical material, 2008.3), PDF p. 7

printed p. 10, SAE J403 NOV.2001. The source table does not specify the analysis type. Manufacturer-range data, not a standard-guaranteed value or heat-lot test, and not a representation of our supply. Condition: Si is an optional value subject to agreement as stated in the source; do not select by default or merge into one broad range. Until selected, do not use it in a complete calculation or assessment. Pb 0.15–0.35 and B 0.0005–0.0030 are optional additions with L/B designation; do not add them automatically to ordinary grades. Special low-P/S quality requires separate agreement verification.

Composition conditions

Verification notes

Grouped tables were expanded in full and checked against original images and notes. Ordinary, residual and conditional elements are kept separate; suffix tables lacking complete base-steel composition are excluded.

1030 · CHINA STEEL CORPORATION · Bars and Wire Rods Product Catalogue 2014-C1 / 7.1.15 SAE · Carbon steels (Edition unspecified)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Bars and wire rod
Original record status
Manufacturer source verified
Document edition
CAT.NO.3-BD-01-2014-C1 (stated on the back cover)
Document title
Bars and Wire Rods Product Catalogue
Table / clause
7.1.15 SAE · Carbon steels (Edition unspecified)
PDF page references
22
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
CHINA STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.3800–0.4900Known-element contribution; incomplete value; missing Cr, Mo, V, Ni, Cu; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300Known-element contribution; incomplete value; missing Mo, Cr, Cu, Ni; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

China Steel bar and wire rod catalogue CAT.NO.3-BD-01-2014-C1, PDF p. 22

printed p. 20, §7.1.15 SAE carbon steels (edition not marked). The source table does not specify the analysis type. Historical manufacturer range data, not a standard-guaranteed value or heat-lot test, and not a representation of our supply. Conditions: Si is an agreement-based option, with separate options for bar and wire rod; B is not automatically added to the ordinary grades in the source table. Where Cu is specified, it is generally ≥0.20%; this is not a default Cu minimum for all steels.

Composition conditions

Verification notes

Merged cells in all 28 catalogue tables were reconstructed geometrically, with no missing cells. Original images, continuation pages and notes are recorded; disputed conditions are withheld.

1030 · ASTM A29/A29M-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
ASTM A29/A29M-2023
Table / clause
Table 1, footnotes A–G
PDF page references
4
Unit
Mass fraction (wt%)
Analysis type
Heat analysis (composition ranges and limits in the original table)

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3850Known-element contribution; incomplete value; missing Si, Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under Table 1 note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3100–0.3883 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under Table 1 note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3133–0.3917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under Table 1 note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.3967 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under Table 1 note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3167–0.3983 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under Table 1 note B
IIW / CEV:0.3800–0.4900 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3200–0.4050 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4300 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Si, Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si ≤0.1% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3200Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.1–0.2% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3233Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.15–0.35% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3250Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.2–0.4% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3267Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Order explicitly adopts Si 0.3–0.6% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C
IIW / CEV:≥ 0.3933Known-element contribution; incomplete value; missing Cr, Mo, V, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):≥ 0.3300Known-element contribution; incomplete value; missing Cr, Ni, Mo, V, B; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:≥ 0.3500Known-element contribution; incomplete value; missing Mo, Cr, Ni; Cu has no specified upper limit; the carbon-equivalent upper bound cannot be determined CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

ASTM A29/A29M-2023 original Table 1: base entries are ladle-analysis mass fraction wt%; product-analysis tolerances are checked separately under 4.3 and Table 5, not added to ladle limits. Orders by Table 1 grade must meet its ladle limits under 4.1.1; other ordered chemistries are separately agreed under 4.1.2 and Tables 3/4 and must not be mixed into this table. General hot-wrought bar requirements do not, by chemistry alone, establish cold-heading suitability, supply or mechanical properties. Note B: the Si range is a common option only when required by the order; Si is unspecified by default, not a universal range or zero. Note C: Cu≥0.20% applies only when expressly required by the order and has no added upper limit. Note D: leaded steel Pb is 0.15–0.35%; retain L as part of the grade identity, not ordinary grades. If lead is added to the ladle stream, its cast or ladle-analysis value cannot be determined. Note F: Bi/Ca/Se/Te are specified by buyer-supplier agreement; do not enter zero when no value is given. Note E: only for expressly specified boron treatment of killed steel, expected B is 0.0005–0.003%; where usual Ti addition is not permitted, up to 0.005% may be expected. These are not mandatory B limits for all ordinary grades.

Original condition-branch records

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Order explicitly adopts Si ≤0.1% under Table 1 note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)

Order explicitly adopts Si 0.1–0.2% under Table 1 note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2

Order explicitly adopts Si 0.15–0.35% under Table 1 note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35

Order explicitly adopts Si 0.2–0.4% under Table 1 note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4

Order explicitly adopts Si 0.3–0.6% under Table 1 note B

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6

Si not otherwise specified in the order; Table 1 does not specify Si, which is not treated as zero;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si ≤0.1% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si≤ 0.1 (lower limit not stated)
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.1–0.2% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.1 ~ 0.2
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.15–0.35% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.15 ~ 0.35
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.2–0.4% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.2 ~ 0.4
Cu≥ 0.2 (upper limit not stated)

Order explicitly adopts Si 0.3–0.6% under Table 1 note B;order explicitly specifies Cu≥0.20% under note C

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)
Si0.3 ~ 0.6
Cu≥ 0.2 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

Existing OCR of the four-page, 190-row original 2023 table was parsed cell by cell. All values were screened for differences against independent 2012 data and checked against the original 2023 images and footnotes; no values were filled from the older edition.

1030 · ASME SA-513

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.27 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A29/A29M-2005

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Cu≤ 0.2 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A510/A510M-2013

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A513/A513M-2025

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A519/A519M-2024

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.04 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A866-2014

Original-source verification is incomplete; this is not a formal standard reference

Material category
Bearing steel
Subcategory
Bearing steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
Al≤ 0.05 (lower limit not stated)
C0.28 ~ 0.34
Cu≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
O≤ 0.002 (lower limit not stated)
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Si0.15 ~ 0.35

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A866-2018

Original-source verification is incomplete; this is not a formal standard reference

Material category
Bearing steel
Subcategory
Bearing steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
Al≤ 0.05 (lower limit not stated)
C0.28 ~ 0.34
Cu≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
O≤ 0.002 (lower limit not stated)
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Si0.15 ~ 0.35

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · U.S. standard

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.05 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A684/A684M-2024

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

1030 · ASTM A684/A684M-2025

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.28 ~ 0.34
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

WhatsApp Technical enquiry →