产品中心/ISO 4954

MATERIAL DATA · COLD FORMING

17Cr3 冷镦钢丝

17Cr3 冷镦钢丝技术资料,执行标准为 ISO 4954。查看当前牌号的化学成分、力学性能及相关技术要求。

供货与技术评审 · 睿雄集团受理本产品的供货与技术评审需求;规格、交货状态、数量和检验文件经评审后按订单技术协议确认。

17Cr3 冷镦钢丝 产品图片
17Cr3 · 冷镦钢丝
01执行标准ISO 4954
02材料牌号17Cr3
03材料形态冷镦钢丝
04交货说明按订单技术条件确认

材料技术参数

1.交货条件的组合

表B.1-交货时热处理条件、产品形式和适用要求的组合

原文表头对照:Heat-treatment condition at delivery=交货热处理状态;Symbol=符号;Wire rod=盘条;Bar=棒材;Wire=钢丝。原标准表格、符号及适用条件保留如下。

Heat-treatment condition at deliverySymbolProducts form aApplicable requirements in cases where the steel concerned has been ordered with reference to the steel names indicated in
Wire rodBarWireT a b les B. 2,B.3,B.4 or B.5Ta bles B. 2,B.3,B.4,B.5,B.6 or B,7Optional
As hot-rolled or peeled+AR or +PEXXXChemical composition as specified in Table B.2Mechanical properties as specified in Ta b le s B.3 ,B.4 and B.5Chemical compositior as specified in Table B.2Mechanical properties as specified in Tables B,3, B.4 and B.5Values for hardenability according to Ta ble s B.6 and B.7Supplementa- ry or special requirements as specified in Annex Eh
Cold drawn+AR+C-XX
Cold drawn + spheroidized+AR+C+AC-XX
Cold drawn + spheroidized+skin passed+AR+C+AC +LC-XX
Spheroidized or spheroidized+peeled+AC or +AC +PEXXX
Spheroidized+cold drawn+AC+CXX
Treated to ferrite- pearlite structure and hardness range+FP-X-
OthersOther delivery conditions may be agreed at the time of ordering
a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order.

2.化学组成

表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)

Steel name b% mass fraction a
CSi cMnPSCrNiMoBCu
17Cr30,12 to 0,200,300,60 to 0,900,0250,0250,70 to 1,25———0,25
Elements not quoted in this table should not be intentionally added to the steel without the agreement of the purchaser,except those intended for finishing the heat.All reasonable precautions shall be taken in order to prevent the addition of such elements from scrap or other materials used in the production process,which can affect the hardenability, mechanical properties and applicability To improve the performance of cold heading,it is possible to add Al:0,020 %to 0,050 % a Maximum values unless otherwise indicated. b In the case of steels with hardenability requirements (see Tables B.6 and B.Z),minor deviations from the specified limits are permitted (with the exception of sulfur and phosphorus),provided that they do not exceed 0,01 %for carbon and the values indicated in Table 2 for the other elements. c A lower silicon content or a specific silicon range may be agreed at the time of ordering

表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)

3.力学性能

表B.5-合金钢牌号的力学性能

Steel nameDiameterDelivery condition
+AC+FP+AR+C+AC+AR+C+AC+LC+AC+C
above mmup to mmRm max. MPaZa min %HB Min.max.Rm max. MPaZ min %Rm max. MPaZ min. %Rm max. MPaZ min. %
17Cr3 17CrS3255206256060
51052060140187500625406063057
104052060140187500625406062057

4.淬透性要求

表B.6-标准淬透性钢种的硬度限值 (H级)

ISO 4954:2018 Table B.6 PDF p.35
Steel nameSymbolAustenitizing temperature ℃±5℃Limits of rangeHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)ofHardness HRC at a distance from quenched end of test piece(in mm)of
Steel nameSymbolAustenitizing temperature ℃±5℃Limits of range1.535791113152025303540
17Cr3+H880max.47444033292725242321———
17Cr3+H880min.39352520—————————

表B.6-标准淬透性钢种 (H级) 的硬度限值 (续)

表B.7-具有限制淬透性散射带的钢种的硬度限值 (HH和HL等级)

Steel nameSymbolAustenitizing temperature ℃±5℃Limits of rangeHardness HRC at a distance from quenched end of test piece(in mm)of
1,535791113152025303540
17Cr3 17CrS3+HH880max.47444033292725242321———
min.4238302420———————
+HLmax.4441352925232120——
min.39352520——
min.42403834312826252220——
min.3937343027242221————

表B.7-淬透性受限的钢种分散带 (HH和HL等级) 的硬度限值 (续)

使用与订购说明

化学成分、力学性能、交货状态及其他技术要求应以现行有效标准、客户图纸和订单技术协议为准;网页资料不替代正式质量证明文件。

询盘建议提供资料

碳当量计算器 — 17Cr3

依据: ISO 4954

化学成分依据: ISO 4954:2018

按所列标准原文转录

产品未注明标准年份;成分采用此处明确列出的已核原文版本。订单适用版本须另行确认,不能推定其他版本相同。

来源原文

Table B.2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15已知项贡献,非完整值: 0.3600–0.6167

缺少元素: Mo, V, Ni

IIW/CEV:碳钢和低合金钢的焊接性初筛。

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B已知项贡献,非完整值: 0.1850–0.3300

缺少元素: Ni, Mo, V, B

Pcm:主要适用于低碳低合金钢;尤其 C 超过 0.11% 时,须另行确认适用性。

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40已知项贡献,非完整值: 0.2150–0.3650

缺少元素: Mo, Ni

CET:铁素体钢焊接预热评估,须核对 EN 1011-2 的适用条件。

单侧上限表示从 0 到该上限;只有下限时不能确定上界。缺项未知,不按零处理。标准极限组合值不是炉批实测值。

碳当量辅助评估焊接性,不代表冷镦、紧固件强度或焊接工艺获准。上述公式不直接适用于不锈钢、铸铁及有色金属。

方法引用: TWI

碳当量计算器 →

提交该材料技术询盘

联系技术团队 →

材料参考资料

同牌号参考不代表标准等同、实际供货或替代批准。

17Cr3 · ISO 683-3:2022

化学成分 · 熔炼分析

质量分数%;表3,用户PDF第17页。未列元素不能当作0;未列元素的有意添加须按标准及订货协议处理。

元素质量分数 / %
C0.12~0.2
Si≤0.4
Mn0.6~0.9
P≤0.025
S≤0.035
Cr0.7~1.25
Cu≤0.4

订货明确采用A.4时,可约定Si≥0.15%;基本表仍为Si≤0.40%。

交货状态与硬度 · 表7

布氏硬度。+S为改善剪切性处理,+A为软化退火,+TH为规定硬度范围处理,+FP为铁素体-珠光体组织处理,+N为正火。“—”为该交货状态未规定要求。

交货状态布氏硬度要求
+S—
+A≤174
+TH—
+FP—
+N—

热处理与试棒条件 · 表8

项目温度 / ℃
末端淬火试验奥氏体化温度880 ± 5
渗碳温度(指导值)880~980
直接及一次淬火温度(指导值)820~860
二次淬火:心部淬火温度(指导值)860~900
二次淬火:表层淬火温度(指导值)780~820
回火温度(指导值)150~200

除末端淬火试验奥氏体化温度外,渗碳、淬火和回火温度均为指导值,实际工艺以达到所需性能为准。奥氏体化时间指导值至少30分钟,回火时间至少1小时。淬火介质按产品形状、冷却条件和装炉量等选择。

淬透性条件 · 表5、表6

距淬火端距离单位为mm;硬度为HRC。仅在订单规定相应淬透性条件时使用。“—”为该位置未规定边界。

+H · 正常淬透性
边界 / 距离mm1.535791113152025303540
最大值47444033292725242321———
最小值39352520—————————
+HH · 窄淬透性带
边界 / 距离mm1.535791113152025303540
最大值47444033292725242321———
最小值4238302420————————
+HL · 窄淬透性带
边界 / 距离mm1.535791113152025303540
最大值4441352925232120—————
最小值39352520—————————
成品分析允许偏差 · 表4
元素熔炼分析规定范围 / %成品分析允许偏差 / %
C0.07<C≤0.31±0.02
Si≤0.40±0.03
Mn≤1.00 / >1.00~1.65±0.04 / ±0.06
P≤0.025+0.005
S≤0.040±0.005
Cr≤1.80±0.05
Mo≤0.30 / >0.30~0.50±0.03 / ±0.04
Ni≤1.00 / >1.00~2.00 / >2.00~3.50±0.03 / ±0.05 / ±0.07
Cu≤0.40+0.05
B≤0.0050±0.0003

“±”表示同炉只能在上限之上或下限之下一个方向偏离,不能同时两向偏离。成品分析偏差不改变表3熔炼分析限值。

标准版次及订货说明

标准涵盖盘条等产品;成品冷镦线供货、工艺及性能按技术评审与订单确认。—表示本表未规定,不能当作0。

来源对照复核:Codex依据用户提供标准原文核对;网页不替代正式标准、订单协议或质量证明文件。

ISO 683-3:2022全部牌号 →