X38CrMo16 material reference
2 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for X38CRMO16 →Material demand assessment
Looking for X38CRMO16 material?
Not listed in our catalog? You are welcome to submit your requirements. We assess whether our equipment, production lines and process capabilities suit your grade, product form, dimensions, processing and delivery requirements, then discuss possible processing, trials or supply arrangements.
Feasibility and supply terms are confirmed after technical review. The standard information on this page is not a supply or performance commitment.
Keep your entries and try again later, or contact website@chqwire.net. If you have already received confirmation, do not submit again.
X38CrMo16 · ISO 4957-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 4957-2018
- Table / clause
- Table 4 · Notes a–g
- PDF page references
- 15、16
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Default S≤.030%; Tabulated Ni range
Default S≤.030%; Ni omitted by agreement; no range specified
Agreed S .050–.100%; Tabulated Ni range
Agreed S .050–.100%; Ni omitted by agreement; no range specified
Composition record (conditional branches apply; this is not an unconditional requirement)
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Applicability and limitations
Table 4 heat composition for cold-work alloy tool steels, wt%; Default P/S are each ≤.030%. ; Product-analysis tolerances in Table 5 must not be applied to the default heat-analysis range. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; dashes are not entered as zero. ; Cold-work tool steel does not establish suitability for cold-heading wire; the words “cold work” alone do not justify listing a product in the product centre. ; Note f: by agreement, S .050–.100% applies and Ni may be omitted; An omission does not mean Ni=0.
Original condition-branch records
Default S≤.030%; Tabulated Ni range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Default S≤.030%; Ni omitted by agreement; no range specified
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Agreed S .050–.100%; Tabulated Ni range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | 0.05 ~ 0.1 |
Agreed S .050–.100%; Ni omitted by agreement; no range specified
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| P | ≤ 0.03 (lower limit not stated) |
| S | 0.05 ~ 0.1 |
A condition branch must be selected
YesVerification notes
Official English Table 4 and footnotes visually checked.X38CrMo16 · BS EN ISO 4957:2018
Chemical-composition source verified. Properties and delivery conditions follow the sources and conditions stated here; actual supply and measured heat results are not verified by this reference.
- Material category
- Tool steel
- Product form
- Tool-steel standard reference; product form subject to the order
- Standard edition
- BS EN ISO 4957:2018
- Table / clause
- Table 4 and notes a–g
- Source file
- BS EN ISO 4957-2018-Tool steel.docx
- Units
- Mass fraction (wt%)
- Analysis type
- Cast analysis
Composition (agreed alternatives apply)
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Default S≤.030%; tabulated Ni range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Default S≤.030%; Ni omitted by agreement, with no specified range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Agreed S .050–.100%; tabulated Ni range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| Ni | ≤ 1 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | 0.05 ~ 0.1 |
Agreed S .050–.100%; Ni omitted by agreement, with no specified range
| Element | Composition requirement |
|---|---|
| C | 0.33 ~ 0.45 |
| Si | ≤ 1 (lower limit not stated) |
| Mn | ≤ 1.5 (lower limit not stated) |
| Cr | 15.5 ~ 17.5 |
| Mo | 0.8 ~ 1.3 |
| P | ≤ 0.03 (lower limit not stated) |
| S | 0.05 ~ 0.1 |
Applicability and limitations
Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero. Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking. Permissible product-analysis deviations do not expand the default cast-analysis limits. Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition. Table 4: alloy cold-work tool steels; cast analysis, wt%; default P and S each ≤.030%. Product-analysis deviations in Table 5 must not be applied to the default cast-analysis limits. Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Dashes are not entered as zero. Note f: S .050–.100% may be agreed and Ni may be omitted. Omission does not mean Ni=0. Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Composition and ordering conditions
- Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero.
- Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking.
- Permissible product-analysis deviations do not expand the default cast-analysis limits.
- Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition.
- Table 4: alloy cold-work tool steels; cast analysis, wt%; default P and S each ≤.030%.
- Product-analysis deviations in Table 5 must not be applied to the default cast-analysis limits.
- Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Dashes are not entered as zero.
- Note f: S .050–.100% may be agreed and Ni may be omitted. Omission does not mean Ni=0.
- Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Mechanical properties and delivery condition
| Property | Standard requirements and applicable conditions |
|---|---|
| Usual delivery condition | Quenched and tempered, approximately 300 HBW (Table 4 note e); this is not a maximum annealed hardness. |
Mechanical-property provenance:BS EN ISO 4957:2018 · Table 4 and notes a–g · Standard tables embedded in the Word document supplied by the user
Verification notes
Checked against the standard text and table notes supplied by the user. Applicability to a specific order requires separate confirmation.
Related catalog and standard references
View standard reference information →
A reference link does not confirm supply or interchangeability. Specific requirements need technical confirmation.