SWRCH45K

9 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for SWRCH45K →

Material demand assessment

Looking for SWRCH45K material?

Not listed in our catalog? You are welcome to submit your requirements. We assess whether our equipment, production lines and process capabilities suit your grade, product form, dimensions, processing and delivery requirements, then discuss possible processing, trials or supply arrangements.

Feasibility and supply terms are confirmed after technical review. The standard information on this page is not a supply or performance commitment.

Explore products and processing capabilities

SWRCH45K · JIS G 3507-1-2021

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Carbon-steel wire rod for cold heading and cold extrusion (SWRCH, diameter≤50mm)
Original record status
Original standard verified
Standard edition
JIS G 3507-1:2021
Table / clause
Clause 4/Table 1; Clause 6/Table 2 with residual-element notes; clauses 7/8; Annex JA
PDF page references
1、5、6、7、8、9、12、13
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.5200–0.7033Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5650Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6000Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Si0.1 ~ 0.35

Applicability and limitations

Based on the official Japanese original text Table 1/2 of JIS G3507-1:2021; This clause is for SWRCH raw material wire rod, heat analysis mass fraction wt%, applicable for diameter ≤50mm. SWRCH wire rod and SWCH wire after processing shall be recorded separately; The reference relationship of raw material composition does not equal the automatic interchangeability of grade, form, delivery condition, or mechanical properties, and shall not be used to increase the company's supply commitment. Table 2: R is rimmed steel equivalent class, A is aluminum killed class, K is killed class. Do not fill 0 for the dashes of Si for R and Al for R/K; Elements not listed in the table or indicated by dashes shall not be intentionally added except for the purpose of finishing steelmaking. For all listed grades, residual Cu≤0.30%, Ni≤0.20%, and Cr≤0.20% according to Table 2; Residual element clauses at the bottom of the table shall not be omitted. For Class A, Al≥0.02% shall be registered as Al per the original table, and shall not be converted to other aluminum analysis types. This table shall not be used to extrapolate fixed mechanical properties of wire after processing from wire rod composition; Corresponding finished product standards, processing states, and test conditions must be verified separately. 7.1 Average decarburization depth applies only to SWRCH30K/33K/35K/38K/40K/41K/43K/45K/48K/50K and when inspection is specified by the buyer: for d≤15mm, ferrite/total decarburization are ≤0.02/0.15mm respectively; for 15<d≤25mm, they are ≤0.03/0.20mm; for 25<d≤32mm, they are ≤0.04/0.25mm; d>32mm shall be according to agreement. This requirement does not apply to all grades. For Class A/K, austenitic grain size and non-metallic inclusions are subject to agreed limits only when specified by the purchaser; Unless otherwise specified, use the cleanliness d(%) upper limit determined by the point-count method in JIS G0555 JA.7 for inclusions; do not directly substitute ASTM E45 ratings. Default surface defect depth: A/K≤0.10mm; R is ≤0.20mm when d≤32mm, and according to agreement when d>32mm. Stricter surface quality levels JA.1/JA.2 are adopted by agreement only and cannot be bundled by default. Verify dimensions and out-of-roundness under 8.3 and the referenced JIS G3191; Precision A/B of JA.3 are independent agreement options; agreement precision cannot be treated as a default requirement.

Verification notes

JIS G 3507-1:2021 Table 2 and residual Cu/Ni limits at the foot of the table checked; SWRCH wire rod and processed SWCH wire are shown separately.

SWRCH45K · Q/BQB 517-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Cold-heading steel
Material form
Hot-rolled steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
Q/BQB 517—2023
Table / clause
6.1.1/Table 1, row 47, note a
PDF page references
10
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Source document

Carbon-equivalent reference

IIW / CEV:0.5200–0.7087Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5640Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6010 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.02 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 47; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Verification notes

All 104 rows of Table 1 and 34 rows of Table 2 in the original Q/BQB517:2023 from Baosteel’s official website were checked row by row; not mixed with older editions.

SWRCH45K · JIS G 3507-1-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Carbon steel for cold heading
Material form
Hot-rolled carbon-steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
JIS G 3507-1:2005
Table / clause
Part 1, Table 2 and residual-element notes; Part 2, Table 1 designation / Part 1 material correspondence
PDF page references
4
Unit
Mass fraction (%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.5200–0.7033Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5650Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6000Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)

Applicability and limitations

JIS G 3507-1:2005, row 36 of the complete table; cast-analysis mass fraction %. SWRCH wire rod and SWCH wire are recorded separately. The chemistry of wire in Part 2 is based on the corresponding same-period raw wire rod in Part 1; D/DA wire mechanical properties cannot be inferred from it. Japanese original, Part 1, Table 2: Cr≤0.20%, residual Cu≤0.30%, Ni≤0.20%; dashes are not filled with zero. The Chinese translation incorrectly gives the carbon maximum for SWRCH15K as 0.15 and omits ≤ in the R-category sulphur column; the corresponding Japanese-original values 0.18 and ≤0.040 are retained here. Sources for the 2005 and 2021 editions are kept separate; identical grade names do not establish the contractual edition or supply by our company.

Verification notes

All 38 rows of Table 2 were compared value by value with the 2021 edition of the Japanese original; two layout errors in the Chinese translation were corrected against the Japanese original.

SWRCH45K · JIS G 3507-1-2010

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Carbon steel for cold heading
Material form
Hot-rolled carbon-steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
JIS G 3507-1:2010
Table / clause
Clauses 3 and 5: main text Tables 1 and 2, and residual-element requirements at the end of the table
PDF page references
6、7
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.5200–0.7033Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5650Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6000Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)

Applicability and limitations

JIS G 3507-1:2010 Japanese original, main-text Tables 1/2, row 36, SWRCH45K; cast analysis, mass fraction wt%. SWRCH is carbon steel wire rod feedstock for cold heading; processed SWCH wire requires separate verification under Part 2 and the contract, without inferring delivery condition or mechanical properties. All grades in main-text Table 2 have Cu≤0.30%, Ni≤0.20%, Cr≤0.20%; dashes mean unspecified, not filled with 0. R is the category equivalent to rimmed steel, A aluminium-killed steel, K killed steel; Al≥0.02% applies only to A, not across categories. Clause 6.1 decarburization testing applies only to SWRCH30K—50K when specified by the purchaser; Clause 6.2 grain/inclusion requirements follow mutual agreement when specified. Historical edition 2010 is shown separately; identical grade names in 2005 and 2021 do not verify the actual contract edition or current supply.

Verification notes

All 38 rows in Tables 1 and 2 of the original 2010 Japanese edition were checked row by row; particular checks covered the sulfur limit for R grades, carbon in 15K, and manganese in 24K/41K.

SWRCH45K · Q/ZNGF 01.7—2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
2023 Edition; Published 2023-09-21, implemented 2023-10-01; Supersedes Q/SG18—2022
Document title
Steel wire rod for cold heading and cold extrusion
Table / clause
Table 1
PDF page references
5
Unit
Mass fraction (wt%)
Manufacturer
Guangdong Zhongnan Iron & Steel Co., Ltd.

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.5200–0.6967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5600Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.5950Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)

Applicability and limitations

Zhongnan Steel Q/ZNGF 01.7—2023, Table 1, row 33 (PDF page 5), cast analysis wt%; footnotes, delivery process and orders must be confirmed against the corresponding edition. This does not constitute a supply commitment by Creation Group.

Composition conditions

Verification notes

2023 edition: all 69 rows of Table 1 and notes a/b/c checked line by line; process suffixes -1/-2/-3 distinguished from footnote letters.

SWRCH45K · BEXG 021-2020

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
BEXG 021-2020, sixteenth revision stated on the cover; issued and effective on 2020-12-29; The latest original document available on this computer only
Document title
Technical delivery conditions for cold-heading steel wire rod for automotive parts
Table / clause
Table 1
PDF page references
4
Unit
Mass fraction (wt%)
Manufacturer
Baoshan Iron & Steel Co., Ltd. (Baosteel)

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.5400–0.7087Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4583–0.5640Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4850–0.6010 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr0.1 ~ 0.2
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Baosteel BEXG 021-2020, Table 1, row 12, PDF page 4; heat-analysis composition in wt%, hot-rolled wire rod. 2020 is the original edition available locally, with no claim that it is the company’s current latest edition. Special conditions and actual supply require separate confirmation.

Composition conditions

Verification notes

Table 1 original images checked page by page, physical pages 3–10; continuation values and other columns kept separate; two disputed rows excluded.

Source footnotes

-

SWRCH45K · POSCO wire rod catalogue (local archive 1203; original edition not stated)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Local file 1203 (wire-rod pdf); the original does not state a publication edition; PDF metadata 2014-12-03 is only the file generation time
Document title
Wire rod
Table / clause
Printed page 20, composition table 1 (local table index)
PDF page references
11
Unit
Percentages as stated in the original table; refer to the source for the specific basis
Analysis type
The catalog does not consistently specify heat or product analysis
Manufacturer
POSCO

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.5200–0.6300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5367 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.5700 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

Locally held POSCO wire rod catalogue, PDF page 11

printed page 20, table index 0, row 29. The original edition number is not stated. The PDF creation date 2014-12-03 is not a standard publication year. Manufacturer range data do not constitute our company’s supply guarantee.

Composition conditions

Verification notes

The original PDF tables and text coordinates were reconciled in both directions. Missing grade cells were restored; merged cells, footers and remarks were checked separately. Tables with identified disputes and rows without composition data are withheld.

SWRCH45K · Nippon Steel Wire Rods EXE203 2008.3 / JIS G3507-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Cat. No. EXE203 2008.3 PDF; cover copyright 2008
Document title
Nippon Steel Wire Rods
Table / clause
Printed page 15, table index 1
PDF page references
9
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
NIPPON STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.5200–0.7033Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5650Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6000Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)

Applicability and limitations

Historical Nippon Steel wire-rod catalogue EXE203 2008.3, PDF page 9

printed page 15, JIS G3507-2005. The original catalogue does not explicitly identify the analysis type for this table. Manufacturer range data, not guaranteed standard limits or heat-specific measurements; this does not establish supply by Creation Group. Condition: the original Aℓ column is retained as Al; R, aluminum-killed and killed classifications follow the original table and are not merged.

Composition conditions

Verification notes

Grouped tables were expanded in full and checked against original images and notes. Ordinary, residual and conditional elements are kept separate; suffix tables lacking complete base-steel composition are excluded.

SWRCH45K · CHINA STEEL CORPORATION · Bars and Wire Rods Product Catalogue 2014-C1 / 7.1.7 JIS G3507-1 (Edition unspecified)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Bars and wire rod
Original record status
Manufacturer source verified
Document edition
CAT.NO.3-BD-01-2014-C1 (stated on the back cover)
Document title
Bars and Wire Rods Product Catalogue
Table / clause
7.1.7 JIS G3507-1 (Edition unspecified)
PDF page references
15
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
CHINA STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.5200–0.7033Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.4533–0.5650Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4800–0.6000Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.42 ~ 0.48
Si0.1 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)

Applicability and limitations

CSC bars and wire rods catalogue CAT.NO.3-BD-01-2014-C1, PDF page 15

printed page 13; clause 7.1.7 cites JIS G3507-1 (edition not stated). The original catalogue does not specify the analysis type for this table. Historical manufacturer scope data; neither standard guaranteed values nor measured heat analysis, and not evidence of supply by our company.

Composition conditions

Verification notes

Merged cells in all 28 catalogue tables were reconstructed geometrically, with no missing cells. Original images, continuation pages and notes are recorded; disputed conditions are withheld.