← BackMaterial grade directory

S38C

12 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for S38C →

S38C · JIS G4051

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Wire rod
Original record status
Source edition identified; composition verification pending
Standard edition
JIS G 4051-2023
Table / clause
Table 2 and notes a/b; Clause 6

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table limits; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the Cr limit is relaxed to Cr≤0.30%; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr≤0.45%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr≤0.45%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

Composition source: JIS G 4051-2023; the product does not state its edition. Confirm the edition applicable to the contract.

Composition conditions

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Original condition-branch records

Table limits; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: only the Cr limit is relaxed to Cr≤0.30%; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr≤0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45

By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr≤0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45

A condition branch must be selected

Yes

Verification notes

Composition source: JIS G 4051-2023; the product does not state its edition. Confirm the edition applicable to the contract.View associated products →

S38C · JIS G 4051-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS G 4051-2023
Table / clause
Table 2 and notes a/b; Clause 6

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table limits; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the Cr limit is relaxed to Cr≤0.30%; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr≤0.45%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr≤0.45%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

Heat-analysis mass fractions wt%; Product-analysis tolerances follow JIS G0321, Table 3 separately. ; Widening the combined maximum for Cr≤0.30% and Ni+Cr requires agreement between both parties; conditions are selected separately; The individual Ni limit ≤0.20% is not widened by this provision. ; Alloying elements not listed in the table must not be intentionally added except to finish steelmaking; Unspecified values must not be treated as zero in calculations.

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Original condition-branch records

Table limits; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: only the Cr limit is relaxed to Cr≤0.30%; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr≤0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45

By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr≤0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45

A condition branch must be selected

Yes

Verification notes

Verified original Japanese Table 2 and normative Annex JB (2023)

S38C · JIS G 4051-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS G 4051-2005
Table / clause
Table 1 and remark 1–3; Clause 5

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table limits; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the Cr limit is relaxed to Cr<0.30%; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr<0.45%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr<0.45%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

Heat-analysis mass fractions wt%; Product-analysis tolerances follow JIS G0321, Table 3 separately. ; Agreed Cr < 0.30%, total Ni+Cr CK < 0.40%

ordinary < 0.45%; Strictly less than, not including the upper limit value; select separately; The individual Ni limit ≤0.20% is not widened by this provision. ; Unspecified elements cannot be calculated as zero values; This record is based only on the 2005 edition; the new edition cannot be automatically assumed to be the same.

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Original condition-branch records

Table limits; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35
    Upper bound excluded
    No

By agreement between the parties: only the Cr limit is relaxed to Cr<0.30%; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35
    Upper bound excluded
    No

By agreement between the parties: only the combined Ni+Cr limit is relaxed; Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

By agreement between the parties: Cr and the combined Ni+Cr limits are relaxed; Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

A condition branch must be selected

Yes

Verification notes

Original Japanese 2005, Table 1 and remark 1–3 have been checked

S38C · JIS G 4051-2016

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS G 4051-2016
Table / clause
Table 2 and notes a/b; Clause 5
PDF page references
1、6、7、8

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Cr≤0.20%;Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr<0.30%; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Cr≤0.20%;Ni+Cr<0.45%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr<0.30%; Ni+Cr<0.45%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

JSA official English version JIS G4051:2016, line-by-line visual verification of cover and original composition table; Mass fraction wt%, heat analysis. ; Note a: The agreed Cr limit is strictly less than 0.30%.; Note b: The agreed Ni+Cr combined limit is strictly less than 0.45%; do not treat it as less than or equal to.; The two agreements are selected independently. ; If product analysis is agreed by both parties, apply the deviations in JIS G0321 Table 3 separately; do not automatically add them to the default heat-analysis range.. ; Elements not listed shall not be intentionally added except additions needed to finish steelmaking; An unspecified limit does not mean that the content is zero.. ; This record is based solely on the 2016 edition; it does not claim that compositions of other editions are identical or have been verified.

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Original condition-branch records

Cr≤0.20%;Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: Cr<0.30%; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Cr≤0.20%;Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

By agreement between the parties: Cr<0.30%; Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

A condition branch must be selected

Yes

Verification notes

Visual check of Table 2 and normative Annex JB, all 27 grades and footnotes, in the official 2016 English original

S38C · JIS G 4051-2016

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS G 4051-2016
Table / clause
Table 2 and notes a/b; Clause 5
PDF page references
1、6、7、8

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Cr≤0.20%;Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr<0.30%; Ni+Cr≤0.35%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Cr≤0.20%;Ni+Cr<0.45%
IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
By agreement between the parties: Cr<0.30%; Ni+Cr<0.45%
IIW / CEV:0.4500–0.6533Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.5000Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5350Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

JSA official English version JIS G4051:2016, line-by-line visual verification of cover and original composition table; Mass fraction wt%, heat analysis. ; Note a: The agreed Cr limit is strictly less than 0.30%.; Note b: The agreed Ni+Cr combined limit is strictly less than 0.45%; do not treat it as less than or equal to.; The two agreements are selected independently. ; If product analysis is agreed by both parties, apply the deviations in JIS G0321 Table 3 separately; do not automatically add them to the default heat-analysis range.. ; Elements not listed shall not be intentionally added except additions needed to finish steelmaking; An unspecified limit does not mean that the content is zero.. ; This record is based solely on the 2016 edition; it does not claim that compositions of other editions are identical or have been verified.

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Original condition-branch records

Cr≤0.20%;Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

By agreement between the parties: Cr<0.30%; Ni+Cr≤0.35%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Cr≤0.20%;Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

By agreement between the parties: Cr<0.30%; Ni+Cr<0.45%

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr<0.3 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Combined limits
Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.45
    Upper bound excluded
    Yes

A condition branch must be selected

Yes

Verification notes

Visual check of Table 2 and normative Annex JB, all 27 grades and footnotes, in the official 2016 English original

S38C · Q/BQB 517-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Cold-heading steel
Material form
Hot-rolled steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
Q/BQB 517—2023
Table / clause
6.1.1/Table 1, row 35, note a
PDF page references
9
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Source document

Carbon-equivalent reference

IIW / CEV:0.4500–0.6387Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4940Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5310 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.02 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 35; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Verification notes

All 104 rows of Table 1 and 34 rows of Table 2 in the original Q/BQB517:2023 from Baosteel’s official website were checked row by row; not mixed with older editions.

S38C · BEXG 021-2020

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
BEXG 021-2020, sixteenth revision stated on the cover; issued and effective on 2020-12-29; The latest original document available on this computer only
Document title
Technical delivery conditions for cold-heading steel wire rod for automotive parts
Table / clause
Table 1
PDF page references
5
Unit
Mass fraction (wt%)
Manufacturer
Baoshan Iron & Steel Co., Ltd. (Baosteel)

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4500–0.6387Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4940Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5310 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Baosteel BEXG 021-2020, Table 1, row 31, PDF page 5; heat-analysis composition in wt%, hot-rolled wire rod. 2020 is the original edition available locally, with no claim that it is the company’s current latest edition. Special conditions and actual supply require separate confirmation.

Composition conditions

Verification notes

Table 1 original images checked page by page, physical pages 3–10; continuation values and other columns kept separate; two disputed rows excluded.

Source footnotes

-

S38C · POSCO wire rod catalogue (local archive 1203; original edition not stated)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Local file 1203 (wire-rod pdf); the original does not state a publication edition; PDF metadata 2014-12-03 is only the file generation time
Document title
Wire rod
Table / clause
Printed page 23, composition table 2 (local table index)
PDF page references
12
Unit
Percentages as stated in the original table; refer to the source for the specific basis
Analysis type
The catalog does not consistently specify heat or product analysis
Manufacturer
POSCO

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

POSCO local wire rod catalogue, PDF page 12

printed page 23, table index 1, row 12. The original edition number is not stated; the PDF creation date 2014-12-03 is not the standard publication year. Manufacturer range information does not constitute our supply guarantee. Printed page 23 footnote: for the three CK grades, upper limits Cu/Ni/Cr/Ni+Cr are 0.25/0.20/0.20/0.30%; for other grades 0.30/0.20/0.20/0.35%. Product-analysis tolerances require separate verification under cited JIS G0321 Table 2; the cited edition is not claimed as checked.

Composition conditions

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Verification notes

The original PDF tables and text coordinates were reconciled in both directions. Missing grade cells were restored; merged cells, footers and remarks were checked separately. Tables with identified disputes and rows without composition data are withheld.

S38C · Nippon Steel Wire Rods EXE203 2008.3 / JIS G4051-2005

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Cat. No. EXE203 2008.3 PDF; cover copyright 2008
Document title
Nippon Steel Wire Rods
Table / clause
Printed page 16, table index 0
PDF page references
10
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
NIPPON STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)

Applicability and limitations

Historical Nippon Steel wire-rod catalogue EXE203 2008.3, PDF page 10

printed page 16, JIS G4051-2005. The original catalogue does not explicitly identify the analysis type for this table. Manufacturer range data, not guaranteed standard limits or heat-specific measurements; this does not establish supply by Creation Group. Condition: residual Cu≤0.25 and Ni+Cr≤0.30 for the three CK grades; Other ≤0.30/0.35; Each Ni≤0.20 and Cr≤0.20.

Composition conditions

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Verification notes

Grouped tables were expanded in full and checked against original images and notes. Ordinary, residual and conditional elements are kept separate; suffix tables lacking complete base-steel composition are excluded.

S38C · Nippon Steel Wire Rods EXE203 2008.3 / JASO M106-92

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
Cat. No. EXE203 2008.3 PDF; cover copyright 2008
Document title
Nippon Steel Wire Rods
Table / clause
Printed page 20, table index 0
PDF page references
12
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
NIPPON STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

Nippon Steel wire-rod catalogue EXE203 2008.3, historical material; PDF p. 12

printed p. 20; JASO M106-92. The original catalogue does not specify the analysis type for this table. Manufacturer range data; not a standard guarantee or a heat-lot test, and does not represent our supply.

Composition conditions

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Lower limit
    Not stated
    Upper limit
    0.35

Verification notes

Grouped tables were expanded in full and checked against original images and notes. Ordinary, residual and conditional elements are kept separate; suffix tables lacking complete base-steel composition are excluded.

S38C · CHINA STEEL CORPORATION · Bars and Wire Rods Product Catalogue 2014-C1 / 7.1.9 JIS G4051 (Edition unspecified)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Bars and wire rod
Original record status
Manufacturer source verified
Document edition
CAT.NO.3-BD-01-2014-C1 (stated on the back cover)
Document title
Bars and Wire Rods Product Catalogue
Table / clause
7.1.9 JIS G4051 (Edition unspecified)
PDF page references
18
Unit
Mass fraction (%)
Analysis type
The original catalogue does not explicitly identify the analysis type for this table
Manufacturer
CHINA STEEL CORPORATION

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4500–0.6333Known-element contribution; incomplete value; missing Mo, V; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4950Known-element contribution; incomplete value; missing Mo, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4100–0.5300Known-element contribution; incomplete value; missing Mo; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.35 ~ 0.41
Si0.15 ~ 0.35
Mn0.6 ~ 0.9
P≤ 0.03 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

CSC bars and wire rods catalogue CAT.NO.3-BD-01-2014-C1, PDF page 18

printed page 16; clause 7.1.9 cites JIS G4051 (edition not stated). The original catalogue does not specify the analysis type for this table. Historical manufacturer scope data; neither standard guaranteed values nor measured heat analysis, and not evidence of supply by our company.

Composition conditions

Combined limits

Element-sum limits
  • Elements concerned
    • Ni
    • Cr
    Upper limit
    0.35

Verification notes

Merged cells in all 28 catalogue tables were reconstructed geometrically, with no missing cells. Original images, continuation pages and notes are recorded; disputed conditions are withheld.

S38C · Q/BQB 615-2018

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.35 ~ 0.41
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
Ni≤ 0.2 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Si0.15 ~ 0.35

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

WhatsApp Technical enquiry →