S32101
22 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for S32101 →S32101 · ASTM A955/A955M-2020(c)
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ASTM A955/A955M-2020(c)
- Table / clause
- Table 2 notes A–E; clauses 1.2,1.6,4.1.3/4.1.6,6.1
- PDF page references
- 1、3、4
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Mn | 4.0 ~ 6.0 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1.0 (lower limit not stated) |
| Cr | 21.0 ~ 22.0 |
| Ni | 1.35 ~ 1.7 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Cu | 0.1 ~ 0.8 |
Applicability and limitations
Alloy recorded in this composition: S32101. Table 2 gives heat-analysis composition as mass fraction wt%; values without a specified range are maxima.; Ellipses indicate no requirement; do not supplement with zero.. ; UNS alloy types and Grade strength levels shall be recorded separately; 60/75/80 refer to the ksi system, and 420/520/550 refer to the MPa system; alloys shall not be guessed based on strength levels.. ; The name 2205 may correspond to S31803 or S32205; they shall be used separately according to the confirmed UNS, and the two composition ranges shall not be mixed. ; This standard is for concrete reinforcing steel; Do not automatically treat this as a cold-heading product available for supply..
Verification notes
Official English 20c Table 2, footnotes and applicable clauses checked item by item.S32101 · ASTM A240/A240M-2014
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Original record status
- Original-standard record
- Standard edition
- ASTM A240/A240M-2014
- Table / clause
- Table 1 and footnotes A–O
- PDF page references
- 1、4、6
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Mn | 4.0 ~ 6.0 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1.0 (lower limit not stated) |
| Cr | 21.0 ~ 22.0 |
| Ni | 1.35 ~ 1.7 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Cu | 0.1 ~ 0.8 |
Applicability and limitations
Table 1 ladle composition, mass fraction %; a single value without a range or lower limit is a maximum, and unspecified elements are not filled with zero. Cb and Nb are the same element; where both a formula and a fixed limit apply, use the more restrictive limit. This is a plate, sheet and strip standard; suitability for cold-heading wire and actual supply require separate verification. Clause 4.1 also requires applicable provisions of ASTM A480/A480M. This record shows ladle composition from Table 1; it does not mean that A480 or all product acceptance requirements have been fully checked.
Combined limits
- Combined-element limits
- Elements requiring measured values from the same heat
S32101 · ASTM A 276-2006
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A 314-2025
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A1082/A1082M-2016
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A182/A182M-2018
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A182/A182M-2025
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A240/240M-2018
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A240/A240M-2020
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A276/A276M-2017
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A276/A276M-2025
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A479/A479M-2018
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A479/A479M-2025
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A511/A511M-2020
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A511/A511M-2025
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A554-2016
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A554-2026
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A789/A789M-2024
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A790/A790M-2024
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A815/A815M-2024
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A815/A815M-2026
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
S32101 · ASTM A959-2019
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Stainless steel
- Subcategory
- Duplex stainless steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.04 (lower limit not stated) |
| Cr | 21 ~ 22 |
| Cu | 0.1 ~ 0.8 |
| Mn | 4 ~ 6 |
| Mo | 0.1 ~ 0.8 |
| N | 0.2 ~ 0.25 |
| Ni | 1.35 ~ 1.7 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
| Si | ≤ 1 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.