← BackMaterial grade directory

S235J2W

1 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for S235J2W →

S235J2W · EN 10025-5-2004

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Hot-rolled structural steel flat and long products with improved atmospheric corrosion resistance; see original-table form and dimensional limits
Original record status
Original standard verified
Standard edition
EN 10025-5:2004
Table / clause
Tables 1/2/3; 6.2/6.3/7.2
PDF page references
1、5、9、15、16、17
Unit
Mass fraction (wt%)
Analysis type
Ladle analysis

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Flat products / Table 2 heat analysis / fully killed FF and sufficient nitrogen binding require separate verification
IIW / CEV:0.1300–0.4940Known-element contribution; incomplete value; missing Mo; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0425–0.2637Known-element contribution; incomplete value; missing Mo, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0525–0.2737Known-element contribution; incomplete value; missing Mo; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Long products (each P/S +0.005%, only within forms and sizes permitted by the original table) / Table 2 heat analysis / fully killed FF and sufficient nitrogen binding require separate verification
IIW / CEV:0.1300–0.4940Known-element contribution; incomplete value; missing Mo; ordering or conditional requirements remain unresolved CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0425–0.2637Known-element contribution; incomplete value; missing Mo, B; ordering or conditional requirements remain unresolved Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0525–0.2737Known-element contribution; incomplete value; missing Mo; ordering or conditional requirements remain unresolved CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C≤ 0.13 (lower limit not stated)
Si≤ 0.4 (lower limit not stated)
Mn0.2 ~ 0.6
P≤ 0.035 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr0.4 ~ 0.8
Cu0.25 ~ 0.55
Ni≤ 0.65 (lower limit not stated)
Al≥ 0.02 (upper limit not stated)
Nb0.015 ~ 0.06
V0.02 ~ 0.12
Ti0.02 ~ 0.1

Applicability and limitations

Based on the official text of EN10025-5:2004 (published as DIN EN10025-5:2005-02); This clause is based on 2004 edition data and shall not serve as a basis for the 2019 edition. The scope covers hot-rolled weather-resistant structural steel flat and long products; this does not establish suitability for cold-heading wire or wire rod, or any supply guarantee by our company. Chemical Table 2 is heat analysis; Table 3 product analysis is listed separately and checked when required at ordering; product-analysis limits must not be used to widen heat-analysis limits. P/S for long products may be 0.005% higher than each value in Table 2; Therefore, composition conditions for flat products and long products are separated, and this exception shall not be automatically applied to flat products. FN means rimmed steel is not permitted; FF is fully killed and contains sufficient nitrogen-fixing elements; Al≥0.020% is an example from the original text, and other nitrogen-fixing elements and inspection documents must also be verified. The FF row is subject to Table 2 footnote c: at least one or a combination of Al≥0.020, Nb0.015–0.060, V0.02–0.12, and Ti0.02–0.10 shall be adopted; When combined, at least one element must reach the listed lower limit; it is not mandatory for all elements to reach the lower limit simultaneously. The current automated reverse lookup does not verify this metallurgical combination requirement; it is not imposed on FN by default. The default N upper limit for FN is 0.009%; Footnote d applies only to S235J0W/S355J0W; when increased to not exceeding 0.012%, the P maximum value must be reduced by 0.005% for every 0.001% increase in N. The N upper limit exception can only be applied when inspection documents prove total Al≥0.020% or sufficient other nitrogen-fixing elements; it cannot be cancelled by default. The maximum heat CEV given in 7.2.3 is 0.44% for S235 and 0.52% for S355; Formula verified against the official English preview of Clause 7.2.3 of EN10025-1:2004: CEV=C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15; Inspection documents must report all elements in the formula; missing items shall not be treated as 0. The listed values are heat-analysis limits; an envelope of independent element limits or a reverse lookup based on individual elements does not establish CEV compliance. Delivery and testing conditions such as hot-rolled, normalized/normalized-rolled shall be confirmed according to 6.3 and 7.3.1; Normalized sample results do not necessarily represent the properties in the original delivery condition. In Table 4, both columns for Rm at 100mm state 'including 100mm', and the boundaries of the original table overlap.. Rm for the 100mm condition in this batch is not automatically provided for now; ReH/elongation data are retained, and Rm must be verified against applicable errata and agreements. Impact Table 5 is longitudinal; Verify WP impact requirements only when agreed at ordering. Samples ≤12mm and reductions must be verified separately in conjunction with EN10025-1:2004; energy values from the original table shall not be applied to all thin materials.

Original condition-branch records

Flat products / Table 2 heat analysis / fully killed FF and sufficient nitrogen binding require separate verification

ElementComposition requirement
C≤ 0.13 (lower limit not stated)
Si≤ 0.4 (lower limit not stated)
Mn0.2 ~ 0.6
P≤ 0.035 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr0.4 ~ 0.8
Cu0.25 ~ 0.55
Ni≤ 0.65 (lower limit not stated)
Al≥ 0.02 (upper limit not stated)
Nb0.015 ~ 0.06
V0.02 ~ 0.12
Ti0.02 ~ 0.1
Combined limits
Conditional composition lower limit
  • Al
  • Nb
  • V
  • Ti
Conditional requirements in the source
  • Footnote
    Table 2c/6.2.2
    Source conditions
    FF requires at least one or a combination of Al/Nb/V/Ti, with at least one element meeting its specified minimum; This requirement is not imposed on default FN; use of the N exception requires separate evidence of nitrogen binding.
    Automatic evaluation implemented
    No
  • Footnote
    7.2.3
    Source conditions
    Heat analysis from the same heat, CEV≤0.44%; The original 7.2.3 formula for EN10025-1:2004 has been checked; All formula elements from the same heat and inspection documentation are still required; reverse matching does not automatically demonstrate compliance.
    Automatic evaluation implemented
    No
Analysis type
Ladle analysis
Product-form scope
Maximum thickness of flat products (mm)
150
Long-product form
Maximum section size (mm)
40
Maximum bar size (mm)
150
Maximum wire size (mm)
60

Long products (each P/S +0.005%, only within forms and sizes permitted by the original table) / Table 2 heat analysis / fully killed FF and sufficient nitrogen binding require separate verification

ElementComposition requirement
C≤ 0.13 (lower limit not stated)
Si≤ 0.4 (lower limit not stated)
Mn0.2 ~ 0.6
P≤ 0.04 (lower limit not stated)
S≤ 0.034999999999999996 (lower limit not stated)
Cr0.4 ~ 0.8
Cu0.25 ~ 0.55
Ni≤ 0.65 (lower limit not stated)
Al≥ 0.02 (upper limit not stated)
Nb0.015 ~ 0.06
V0.02 ~ 0.12
Ti0.02 ~ 0.1
Combined limits
Conditional composition lower limit
  • Al
  • Nb
  • V
  • Ti
Conditional requirements in the source
  • Footnote
    Table 2c/6.2.2
    Source conditions
    FF requires at least one or a combination of Al/Nb/V/Ti, with at least one element meeting its specified minimum; This requirement is not imposed on default FN; use of the N exception requires separate evidence of nitrogen binding.
    Automatic evaluation implemented
    No
  • Footnote
    7.2.3
    Source conditions
    Heat analysis from the same heat, CEV≤0.44%; The original 7.2.3 formula for EN10025-1:2004 has been checked; All formula elements from the same heat and inspection documentation are still required; reverse matching does not automatically demonstrate compliance.
    Automatic evaluation implemented
    No
Analysis type
Ladle analysis
Product-form scope
Maximum thickness of flat products (mm)
150
Long-product form
Maximum section size (mm)
40
Maximum bar size (mm)
150
Maximum wire size (mm)
60

A condition branch must be selected

Yes

Verification notes

EN10025-5:2004 Table 2 heat analysis composition and Table 1 ranges have been verified; Keep product form, N–P conditions and nitrogen-fixing conditions separate; the CEV formula reference in 7.2.3 has been checked; Rm at 100mm and the general sampling/impact-test references remain unverified.

Product-analysis composition requirements

C
Lower limit
Not stated
Upper limit
0.16
Si
Lower limit
Not stated
Upper limit
0.45
Mn
Lower limit
0.15
Upper limit
0.7
P
Lower limit
Not stated
Upper limit
0.04
S
Lower limit
Not stated
Upper limit
0.035
Cr
Lower limit
0.35
Upper limit
0.85
Cu
Lower limit
0.2
Upper limit
0.6
Ni
Lower limit
Not stated
Upper limit
0.7
Al
Lower limit
0.02
Upper limit
Not stated
Nb
Lower limit
0.01
Upper limit
0.065
V
Lower limit
0.01
Upper limit
0.14
Ti
Lower limit
0.01
Upper limit
0.12

Cold flanging (additional ordering condition)

EN10025-5:2004 · DIN EN10025-5:2005-02 / DIN Handbook402 English text · Table 6 and Notes a/b, 7.4.2.3 (Option 11c) · PDF pages 11, 20

Applies only when expressly required at ordering; For bending angles <90°, values are minimum recommended inside bend radii in mm, not multiples of thickness.

t: bending direction transverse to the rolling direction

Nominal thickness t (mm)Minimum recommended inside bend radius (mm)
1.5 < t ≤ 2.52.5
2.5 < t ≤ 33
3 < t ≤ 45
4 < t ≤ 56
5 < t ≤ 68
6 < t ≤ 710
7 < t ≤ 812
8 < t ≤ 1016
10 < t ≤ 1220
12 < t ≤ 1425
14 < t ≤ 1628
16 < t ≤ 1836
18 < t ≤ 2040

l: bending direction parallel to the rolling direction

Nominal thickness t (mm)Minimum recommended inside bend radius (mm)
1.5 < t ≤ 2.52.5
2.5 < t ≤ 33
3 < t ≤ 46
4 < t ≤ 58
5 < t ≤ 610
6 < t ≤ 712
7 < t ≤ 816
8 < t ≤ 1020
10 < t ≤ 1225
12 < t ≤ 1428
14 < t ≤ 1632
16 < t ≤ 1840
18 < t ≤ 2045
WhatsApp Technical enquiry →