ML20MnVB · GB/T 5953

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Wire rod
Original record status
Reference transcription of standard
Standard edition
GB/T 6478-2015
Table / clause
Table 4

Carbon-equivalent reference

IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2543–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al(total)≥ 0.02 (upper limit not stated)
V0.07 ~ 0.12

Applicability and limitations

Clause 6.1.1 of GB/T5953.1/.2:2009 follows the relevant standards identified in the contract; This is reference composition for the same designation under GB/T6478; the applicable standard must be confirmed by contract, and these values are not directly treated as mandatory composition under 5953. Table 4 Footnote: The lower limit of Si may be agreed to be lower than 0.10%; The lower limit of B may be relaxed to 0.0005% if conditions are met; If acid-soluble Al is determined, use ≥0.0150%. No edition is stated on the website; Displayed under this source edition; contract applicability is not established

Verification notes

Standard source: GB/T 6478-2015 · Table 4View associated products →

ML20MnVB · GB/T 28906-2025

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Boron-containing cold-heading steel for quenching and tempering
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 28906-2025
Table / clause
Table 4 · Footnotes; 7.1.5–7.1.7
PDF page references
10、11

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Determine total aluminum Alt: 0.020–0.060%.
IIW / CEV:0.4107–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2593–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Determine total aluminum Alt: 0.020–0.060%.; Provided hardenability and mechanical requirements are met and both parties agree, the B minimum is 0.0005%
IIW / CEV:0.4107–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2578–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Determine acid-soluble aluminum Als: 0.015–0.055%.
IIW / CEV:0.4107–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2593–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Determine acid-soluble aluminum Als: 0.015–0.055%.; Provided hardenability and mechanical requirements are met and both parties agree, the B minimum is 0.0005%
IIW / CEV:0.4107–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2578–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.3 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al0.02 ~ 0.06

Applicability and limitations

Mass percent, heat analysis, GB/T28906-2025 Table 4. ; 7.1.5 residual Cr/Ni/Cu are each ≤0.20% and Sn≤0.06%; tabulated alloy Cr is not subject to the residual maximum; 7.1.7 product-analysis tolerances follow GB/T222 and must not be directly treated as heat-analysis limits. ; The standard scope for hot-rolled cold-heading wire rod does not replace confirmation of actual supply dimensions and the component manufacturing process; Mechanical properties require separate verification. ; When measuring acid-soluble aluminum, Als0.015–0.055% is used and is retained separately from total aluminum Alt0.020–0.060%; The Al element field must be interpreted with the selected measurement condition. ; Table 4 Note a: A Si lower limit below 0.10% may be negotiated and specified in the contract; do not fill in without agreement. ; Note b: When hardenability and mechanical properties meet requirements and upon mutual agreement, the lower limit of B may be relaxed to 0.0005%; Default 0.0008%. ; Note c: The Ti/N ratio may be agreed upon, but as no uniform value is provided in the original text, it shall not be automatically set or declared as satisfied. ; Note e: Cr may be added by agreement for the first 15 grades, with the addition amount to be confirmed by both parties.

Original condition-branch records

Determine total aluminum Alt: 0.020–0.060%.

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.3 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al0.02 ~ 0.06

Determine total aluminum Alt: 0.020–0.060%.; Provided hardenability and mechanical requirements are met and both parties agree, the B minimum is 0.0005%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.3 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0005 ~ 0.0035
Al0.02 ~ 0.06

Determine acid-soluble aluminum Als: 0.015–0.055%.

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.3 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al0.015 ~ 0.055

Determine acid-soluble aluminum Als: 0.015–0.055%.; Provided hardenability and mechanical requirements are met and both parties agree, the B minimum is 0.0005%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.3 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0005 ~ 0.0035
Al0.015 ~ 0.055

A condition branch must be selected

Yes

Verification notes

Visual check of the original composition table and footnotes

ML20MnVB · GB/T 28906-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Boron-containing cold-heading steel for quenching and tempering
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 28906-2012
Table / clause
Table 4; 6.1.3/6.1.5–6.1.7
PDF page references
6、7

Carbon-equivalent reference

IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2543–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al≥ 0.02 (upper limit not stated)

Applicability and limitations

GB/T28906-2012, Table 4, heat analysis, mass percent. ; Alt in the table is total aluminum, with requirement ≥0.020% but no maximum; the 2025 maximum or acid-soluble-aluminum replacement conditions are not applied. ; 6.1.5 residual Cr/Ni/Cu are each ≤0.20%; Where Cr is a tabulated alloy range, the residual Cr maximum does not apply; Where Sn is unspecified in the original text, the Sn maximum from a newer edition is not inserted. ; 6.1.7 composition tolerances follow GB/T222; Heat-analysis limits are not treated as product-analysis tolerances. ; The standard scope covers hot-rolled cold-heading wire rod; supply conditions and the actual component process still require confirmation. ; Table 4 of 2012 does not list the relaxed B minimum or low-Si agreement in edition 2025; these conditions are not applied across editions.

Verification notes

All original table entries and related notes visually verified

ML20MnVB · GB/T 6478-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Boron-containing cold-heading steel for quenching and tempering
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 6478-2015
Table / clause
Table 4 · Footnotes; 6.1.5–6.1.7
PDF page references
9、10

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Measured total aluminium (Alt) ≥ 0.020%
IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2543–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Measured total aluminium (Alt) ≥ 0.020%; Provided hardenability and mechanical requirements are met, the agreed B minimum is 0.0005%
IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2528–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Measured acid-soluble aluminium (Als) ≥ 0.015%
IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2543–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Measured acid-soluble aluminium (Als) ≥ 0.015%; Provided hardenability and mechanical requirements are met, the agreed B minimum is 0.0005%
IIW / CEV:0.3940–0.5873Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2528–0.3728Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3000–0.4150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al≥ 0.02 (upper limit not stated)

Applicability and limitations

GB/T6478-2015, Table 4, heat-analysis mass percentages. ; 6.1.5 residual Cr/Ni/Cu are each ≤.20%; tabulated alloy Cr is not subject to the residual Cr maximum. ; 6.1.7 product-analysis tolerances follow GB/T222 and do not widen the default heat-analysis range; Where Sn is unspecified, limits from a newer edition are not inserted. ; Specific dimensions, product condition and mechanical-property conditions require separate verification; composition alone does not establish suitability for forming a component. ; Alt is total aluminum ≥.020%; when measuring acid-soluble aluminum, Als≥.015% applies; no maximum is specified; The Al field must be interpreted according to the selected measurement basis. ; Table 4 Note a: the lower limit of Si may be agreed to be lower than .10%; the specific agreed range is unknown and shall not be filled in arbitrarily. ; Note b: when hardenability and mechanical properties meet the requirements, the B lower limit may be relaxed to .0005%; Selecting this condition does not represent that performance verification has been completed.

Original condition-branch records

Measured total aluminium (Alt) ≥ 0.020%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al≥ 0.02 (upper limit not stated)

Measured total aluminium (Alt) ≥ 0.020%; Provided hardenability and mechanical requirements are met, the agreed B minimum is 0.0005%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0005 ~ 0.0035
Al≥ 0.02 (upper limit not stated)

Measured acid-soluble aluminium (Als) ≥ 0.015%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0008 ~ 0.0035
Al≥ 0.015 (upper limit not stated)

Measured acid-soluble aluminium (Als) ≥ 0.015%; Provided hardenability and mechanical requirements are met, the agreed B minimum is 0.0005%

ElementComposition requirement
C0.18 ~ 0.23
Si0.1 ~ 0.3
Mn1.2 ~ 1.6
V0.07 ~ 0.12
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
B0.0005 ~ 0.0035
Al≥ 0.015 (upper limit not stated)

A condition branch must be selected

Yes

Verification notes

Visual check of all relevant ranges and footnotes in original Tables 1, 2, 4 and 5

ML20MnVB · GB/T 6478-2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 6478-2001
Table / clause
Table 4 / 6.1.4–6.1.8
PDF page references
6

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Total aluminum Alt≥.020%
IIW / CEV:0.4040–0.5973Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2595–0.3828Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4250Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Acid-soluble aluminum Als≥.015%
IIW / CEV:0.4040–0.5973Known-element contribution; incomplete value; missing Mo CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2595–0.3828Known-element contribution; incomplete value; missing Mo Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4250Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.19 ~ 0.24
Si≤ 0.3 (lower limit not stated)
Mn1.2 ~ 1.6
B0.0005 ~ 0.0035
Al≥ 0.02 (upper limit not stated)
V0.07 ~ 0.12
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

GB/T6478-2001, Table 4, heat analysis wt%; 6.1.4 residual Cr/Ni/Cu are each ≤.20%; alloy Cr ranges are not subject to the residual maximum. ; 6.1.8 product-analysis tolerances require separate verification under GB/T222-1984, Table 2, and do not widen the default heat-analysis range. ; Actual 2001 edition; Composition from editions 2015 or 2025 is not substituted for this edition; specific dimensions and delivery mechanical properties require separate verification. ; Table 4 total aluminum Alt≥.020%; An acid-soluble aluminum determination satisfying Als≥.015% is also acceptable; Default B in this edition is .0005–.0035%.

Original condition-branch records

Total aluminum Alt≥.020%

ElementComposition requirement
C0.19 ~ 0.24
Si≤ 0.3 (lower limit not stated)
Mn1.2 ~ 1.6
B0.0005 ~ 0.0035
Al≥ 0.02 (upper limit not stated)
V0.07 ~ 0.12
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Acid-soluble aluminum Als≥.015%

ElementComposition requirement
C0.19 ~ 0.24
Si≤ 0.3 (lower limit not stated)
Mn1.2 ~ 1.6
B0.0005 ~ 0.0035
Al≥ 0.015 (upper limit not stated)
V0.07 ~ 0.12
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Visual check of four composition tables and clauses on pages 5 and 6 of the original PDF

ML20MnVB · Q/BQB 517-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Cold-heading steel
Material form
Hot-rolled steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
Q/BQB 517—2023
Table / clause
6.1.1/Table 1, row 97, note a
PDF page references
12
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Source document

Original composition-element notation and analysis basis
Al
Original element symbol
Alₜ
Symbol extracted from the original source
Alt
Original table column heading
Al t
Subscript in the original source
t
Subscript explanation
Only original table subscripts shall be retained; do not expand these into total aluminum or acid-soluble aluminum; Al without specified form shall not be directly equated
Standard edition
Q/BQB 517—2023
Table / clause
1
Original table item number
97
PDF page references
12
Unit
Mass fraction (wt%)
Analysis type
Heat analysis
Original record status
Original column symbol verified
Original cell
≥ 0.020

When the original analysis designations differ, or a record leaves them unspecified, comparability or a match cannot be concluded directly. Subscripts not explained by the source are not expanded here.

Carbon-equivalent reference

IIW / CEV:0.4040–0.6093 Independent-element envelope of standard ranges; not measured heat-analysis values CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2595–0.3868 Independent-element envelope of standard ranges; not measured heat-analysis values Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3100–0.4310 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.19 ~ 0.24
Si≤ 0.3 (lower limit not stated)
Mn1.2 ~ 1.6
P≤ 0.02 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
B0.0005 ~ 0.0035
Alₜ≥ 0.02 (upper limit not stated)
V0.07 ~ 0.12
Cr≤ 0.2 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 97; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Verification notes

All 104 rows of Table 1 and 34 rows of Table 2 in the original Q/BQB517:2023 from Baosteel’s official website were checked row by row; not mixed with older editions.
WhatsApp Technical enquiry →