ML20Al · GB/T 5953

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Wire rod
Original record status
Reference transcription of standard
Standard edition
GB/T 6478-2015
Table / clause
Table 1

Carbon-equivalent reference

IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Al(total)≥ 0.02 (upper limit not stated)

Applicability and limitations

Clause 6.1.1 of GB/T5953.1/.2:2009 follows the relevant standards identified in the contract; This is reference composition for the same designation under GB/T6478; the applicable standard must be confirmed by contract, and these values are not directly treated as mandatory composition under 5953. No edition is stated on the website; Displayed under this source edition; contract applicability is not established

Verification notes

Standard source: GB/T 6478-2015 · Table 1View associated products →

ML20Al · GB/T 28906-2025

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Non-heat-treated cold-heading steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 28906-2025
Table / clause
Table 1 · Footnotes; 7.1.5–7.1.7
PDF page references
7、8、11

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Determine total aluminum Alt: 0.020–0.060%.
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Determine acid-soluble aluminum Als: 0.015–0.055%.
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al0.02 ~ 0.06
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

Mass percent, heat analysis, GB/T28906-2025 Table 1. ; 7.1.5 residual Cr/Ni/Cu are each ≤0.20% and Sn≤0.06%; tabulated alloy Cr is not subject to the residual maximum; 7.1.7 product-analysis tolerances follow GB/T222 and must not be directly treated as heat-analysis limits. ; The standard scope for hot-rolled cold-heading wire rod does not replace confirmation of actual supply dimensions and the component manufacturing process; Mechanical properties require separate verification. ; When measuring acid-soluble aluminum, Als0.015–0.055% is used and is retained separately from total aluminum Alt0.020–0.060%; The Al element field must be interpreted with the selected measurement condition. ; Table 2, note a: the four grades in Table 1, item 8–11 also apply to case-hardening types.

Original condition-branch records

Determine total aluminum Alt: 0.020–0.060%.

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al0.02 ~ 0.06
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Determine acid-soluble aluminum Als: 0.015–0.055%.

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al0.015 ~ 0.055
P≤ 0.025 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Visual check of the original composition table and footnotes

ML20Al · GB/T 28906-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Non-heat-treated cold-heading steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 28906-2012
Table / clause
Table 1; 6.1.3/6.1.5–6.1.7
PDF page references
5、7

Carbon-equivalent reference

IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

GB/T28906-2012, Table 1, heat analysis, mass percent. ; Alt in the table is total aluminum, with requirement ≥0.020% but no maximum; the 2025 maximum or acid-soluble-aluminum replacement conditions are not applied. ; 6.1.5 residual Cr/Ni/Cu are each ≤0.20%; Where Cr is a tabulated alloy range, the residual Cr maximum does not apply; Where Sn is unspecified in the original text, the Sn maximum from a newer edition is not inserted. ; 6.1.7 composition tolerances follow GB/T222; Heat-analysis limits are not treated as product-analysis tolerances. ; The standard scope covers hot-rolled cold-heading wire rod; supply conditions and the actual component process still require confirmation. ; Table 1 of 6.1.3, item 4–11: the eight grades also apply to case-hardening types.

Verification notes

All original table entries and related notes visually verified

ML20Al · GB/T 6478-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Subcategory
Non-heat-treated cold-heading steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 6478-2015
Table / clause
Table 1 · Footnotes; 6.1.5–6.1.7
PDF page references
8、10

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Measured total aluminium (Alt) ≥ 0.020%
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Measured acid-soluble aluminium (Als) ≥ 0.015%
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

GB/T6478-2015, Table 1, heat-analysis mass percentages. ; 6.1.5 residual Cr/Ni/Cu are each ≤.20%; tabulated alloy Cr is not subject to the residual Cr maximum. ; 6.1.7 product-analysis tolerances follow GB/T222 and do not widen the default heat-analysis range; Where Sn is unspecified, limits from a newer edition are not inserted. ; Specific dimensions, product condition and mechanical-property conditions require separate verification; composition alone does not establish suitability for forming a component. ; Alt is total aluminum ≥.020%; when measuring acid-soluble aluminum, Als≥.015% applies; no maximum is specified; The Al field must be interpreted according to the selected measurement basis. ; Table 2 note: the eight grades in Table 1, item 4–11 also apply to case-hardening types.

Original condition-branch records

Measured total aluminium (Alt) ≥ 0.020%

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Measured acid-soluble aluminium (Als) ≥ 0.015%

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.015 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Visual check of all relevant ranges and footnotes in original Tables 1, 2, 4 and 5

ML20Al · GB/T 6478-2001

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 6478-2001
Table / clause
Table 1 / 6.1.4–6.1.8
PDF page references
5、6

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Table 1 default Si≤0.10%
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2867Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Basic electric furnace steelmaking, Si≤0.17%
IIW / CEV:0.2300–0.3967Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.1950–0.2890Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2100–0.3150Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

GB/T6478-2001, Table 1, heat analysis wt%; 6.1.4 residual Cr/Ni/Cu are each ≤.20%; alloy Cr ranges are not subject to the residual maximum. ; 6.1.8 product-analysis tolerances require separate verification under GB/T222-1984, Table 2, and do not widen the default heat-analysis range. ; Actual 2001 edition; Composition from editions 2015 or 2025 is not substituted for this edition; specific dimensions and delivery mechanical properties require separate verification. ; 6.1.5, Table 1: Si≤.17% for aluminum-killed steel made in a basic electric furnace.

Original condition-branch records

Table 1 default Si≤0.10%

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.1 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

Basic electric furnace steelmaking, Si≤0.17%

ElementComposition requirement
C0.18 ~ 0.23
Si≤ 0.17 (lower limit not stated)
Mn0.3 ~ 0.6
Al≥ 0.02 (upper limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Cr≤ 0.2 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

Visual check of four composition tables and clauses on pages 5 and 6 of the original PDF