HSB61-0.8-0.5

1 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for HSB61-0.8-0.5 →

HSb61-0.8-0.5 · GB/T 5231-2012

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Copper and copper alloys
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 5231-2012
Table / clause
Table 3, row 62, designation T68200
PDF page references
9
Unit
Mass fraction (wt%)

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
Cu59.0 ~ 63.0
Fe≤ 0.2 (lower limit not stated)
Pb≤ 0.2 (lower limit not stated)
Sb0.4 ~ 1.2
Si0.3 ~ 1.0
Cd≤ 0.01 (lower limit not stated)

Applicability and limitations

Mass fraction wt%; GB/T 5231-2012, Table 3, row 62, designation T68200; Scanned PDF, page 9. Zn is the balance; A dash means unspecified; it is not entered as zero. Clause 2.2: single tabulated impurity values are maxima. Tabulated total impurities ≤0.5%; verify using measured contents of the impurity elements specified in the standard. This standard provides composition designations for wrought copper and copper alloys; actual supply and cold-heading suitability require separate confirmation. Table 3, note j: the range 0.05–1.2% is for combined Ni+Sn+B, not for Ni alone. Table 3, note c: total impurities are the sum of measured contents of the impurity elements listed in the table.

Combined limits

Combined-element limits
  • Requirement
    Table 3, note j: combined Ni+Sn+B
    Element coefficient
    Ni
    1
    Sn
    1
    B
    1
    Lower limit
    0.05
    Upper limit
    1.2
Elements requiring measured values from the same heat
  • B
  • Ni
  • Sn

Verification notes

The original scanned standard, Table 3 was manually checked cell by cell; Coupled elements and application-specific footnotes require separate verification