G10080
5 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for G10080 →G10080 · SAE J 403-2001
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- SAE J403 NOV2001
- Table / clause
- Table 1 and Notes 1, 2 and *
- PDF page references
- 1、3、4
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Table 1, general applications, including wire rod; Mn .30–.50%
Note *: structural sections, plate, strip, sheet and welded tube; Mn≤.50%, with no minimum
Composition record (conditional branches apply; this is not an unconditional requirement)
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.3 ~ 0.5 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Applicability and limitations
Original Table 1 UNS G10080 corresponds to SAE1008.; The two names are for retrieval correspondence.. ; Heat analysis wt%; Mn has no lower limit for structural sections/steel plates/strips/sheets/welded pipes; this is not automatically applied to wire rod.. ; Si is not a uniform mandatory component; When required, common ranges for bar products/semi-finished products are ≤ .10, .10–.20, .15–.35, .20–.40, .30–.60%; wire rod has a separate range of .07–.15%; No single range has been arbitrarily selected in this record. ; When Cu is required, it is generally specified as ≥.20%, which is not a uniform Cu upper limit or a default requirement. ; Addition of Pb .15–.35% requires L identification and a change to the UNS; Addition of B .0005–.003% requires B identification and shall not be merged into ordinary 1008.. ; Lower P/S for certain qualities/products must be verified separately per J411 and shall not apply agreement values from subsequent years. ; A requirement to report additional elements does not establish uniform limits for those elements in this table.; Unspecified Si/Cr/Ni/Mo etc. shall not be filled as zero; Finished product deviation to be verified separately per J409.
Original condition-branch records
Table 1, general applications, including wire rod; Mn .30–.50%
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.3 ~ 0.5 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Note *: structural sections, plate, strip, sheet and welded tube; Mn≤.50%, with no minimum
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | ≤ 0.5 (lower limit not stated) |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
A condition branch must be selected
YesVerification notes
Official English Table 1 and footnotes visually checked.G10080 · ASTM A29/A29M-2012
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.25 ~ 0.6 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
G10080 · ASTM A29/A29M-2012
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.3 ~ 0.5 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
G10080 · ASTM A29/A29M-2020
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.25 ~ 0.6 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.
G10080 · ASTM A29/A29M-2023
Original-source verification is incomplete; this is not a formal standard reference
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Verification status
- Reference data; original source not verified
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | ≤ 0.1 (lower limit not stated) |
| Mn | 0.25 ~ 0.6 |
| P | ≤ 0.04 (lower limit not stated) |
| S | ≤ 0.05 (lower limit not stated) |
Applicability and limitations
A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.