2 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for C80U →C80U · ISO 4957-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 4957-2018
- Table / clause
- Table2 and note a/b/c
- PDF page references
- 13
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.75 ~ 0.85 |
| Si | 0.1 ~ 0.3 |
| Mn | 0.1 ~ 0.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Applicability and limitations
Table 2 non-alloy cold-work tool steel, heat analysis mass fraction wt%, P/S each ≤.030%. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; Unspecified Cr/Ni etc. shall not be filled as zero. ; Note a: hardness in cold-drawn state +A+C may be 20HBW higher than annealed +A; This review does not treat test temperatures or hardness as universal delivery properties.. ; Tool steel shall not be identified for cold heading purposes based on the name "cold-work"; specific products and forming suitability must be verified separately. ; Note c C70U to C120U are shallow-hardening steels; For a diameter of 30mm, the hardening depth is approximately 3mm; through-hardening may only be achieved for diameters up to 10mm, and is not guaranteed for arbitrary sizes..
Verification notes
All ranges and footnotes in original Table 2 were visually checkedC80U · BS EN ISO 4957:2018
Chemical-composition source verified. Properties and delivery conditions follow the sources and conditions stated here; actual supply and measured heat results are not verified by this reference.
- Material category
- Tool steel
- Product form
- Tool-steel standard reference; product form subject to the order
- Standard edition
- BS EN ISO 4957:2018
- Table / clause
- Table 2 and notes a/b/c
- Source file
- BS EN ISO 4957-2018-Tool steel.docx
- Units
- Mass fraction (wt%)
- Analysis type
- Cast analysis
Composition
| Element | Composition requirement |
|---|---|
| C | 0.75 ~ 0.85 |
| Si | 0.1 ~ 0.3 |
| Mn | 0.1 ~ 0.4 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Applicability and limitations
Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero. Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking. Permissible product-analysis deviations do not expand the default cast-analysis limits. Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition. Table 2: non-alloy cold-work tool steels; cast analysis, wt%; P and S each ≤.030%. Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Unspecified Cr, Ni and other elements are not entered as zero. The term cold-work tool steel does not establish cold-heading suitability. The product and forming application require separate assessment. Note c: C70U to C120U are shallow-hardening steels. A diameter of 30 mm gives a hardened depth of approximately 3 mm; through-hardening may be possible only up to 10 mm diameter. This is not a guarantee for arbitrary dimensions. C70U–C120U are shallow-hardening steels: at 30 mm diameter, hardened depth is approximately 3 mm; through-hardening may be possible only at diameters not exceeding 10 mm. Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Composition and ordering conditions
- Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero.
- Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking.
- Permissible product-analysis deviations do not expand the default cast-analysis limits.
- Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition.
- Table 2: non-alloy cold-work tool steels; cast analysis, wt%; P and S each ≤.030%.
- Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Unspecified Cr, Ni and other elements are not entered as zero.
- The term cold-work tool steel does not establish cold-heading suitability. The product and forming application require separate assessment.
- Note c: C70U to C120U are shallow-hardening steels. A diameter of 30 mm gives a hardened depth of approximately 3 mm; through-hardening may be possible only up to 10 mm diameter. This is not a guarantee for arbitrary dimensions.
- C70U–C120U are shallow-hardening steels: at 30 mm diameter, hardened depth is approximately 3 mm; through-hardening may be possible only at diameters not exceeding 10 mm.
- Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Mechanical properties and delivery condition
| Property | Standard requirements and applicable conditions |
|---|---|
| Annealed hardness HBW / maximum | 192 |
| Hardening test | Austenitizing 790±10 °C ; water quenching ; 180±10 °C tempering ; hardness≥58 HRC |
Mechanical-property provenance:BS EN ISO 4957:2018 · Table 2 and notes a/b/c · Standard tables embedded in the Word document supplied by the user
Verification notes
Checked against the standard text and table notes supplied by the user. Applicability to a specific order requires separate confirmation.