C10E
3 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for C10E →C10E · DIN EN 10084-2008
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- DIN EN 10084-2008
- Table / clause
- Table 3, notes a–d
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.07 ~ 0.13 |
| Si | ≤ 0.4 (lower limit not stated) |
| Mn | 0.3 ~ 0.6 |
| P | ≤ 0.035 (lower limit not stated) |
| S | ≤ 0.035 (lower limit not stated) |
Applicability and limitations
Ladle analysis, mass fraction wt%; the DIN EN 10084:2008-06 cover expressly identifies the German edition of EN 10084:2008; Table 3 follows that source text. Note b: minor composition deviations associated with hardenability requirements must be checked separately against Table 4 and the applicable conditions; they do not widen default ranges, and no such relaxation applies to P/S. Note c: higher S (approximately up to 0.10%) or Pb may be requested for improved machinability; in the higher-S case, the Mn upper limit may increase by 0.15 percentage points. Actual agreed values are not given; do not invent them or apply them automatically. Note d: B in this table improves toughness in the hardened case, not hardenability. Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); unspecified does not mean zero. A delivery standard for case-hardening steel does not mean all conditions are suitable for cold heading; verify mechanical properties, hardness and hardenability separately.
Verification notes
Original German Table 3 and its footnotes checkedC10E · EN 10132-2-2000
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Cold-rolled narrow strip; dimensions and delivery condition subject to applicable conditions
- Original record status
- Original standard verified
- Standard edition
- EN 10132-2:2000
- Table / clause
- Table 1; Table 2; clauses 1,4,7.3–7.5
- PDF page references
- 1、4、5、7
- Unit
- Mass fraction (wt%)
- Analysis type
- Heat analysis
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.07 ~ 0.13 |
| Si | ≤ 0.4 (lower limit not stated) |
| Mn | 0.3 ~ 0.6 |
| P | ≤ 0.035 (lower limit not stated) |
| S | ≤ 0.035 (lower limit not stated) |
| Cr | ≤ 0.4 (lower limit not stated) |
Applicability and limitations
Actually based on the official English text of EN 10132-2:2000; This standard covers cold-rolled narrow steel strip intended for heat treatment; it does not constitute a supply guarantee for cold-heading wire.. Table 1 is for heat analysis; Permissible deviations for finished product analysis in Table 2 are registered independently; finished product permissible deviations shall not be used to relax heat analysis. Table 1 Footnote: Elements not listed shall not be intentionally added without the buyer's consent, except additions needed to finish steelmaking; Prevent scrap or other raw materials from introducing elements that could impair properties or intended use; unlisted elements must not be assumed zero.. Values in Mechanical Table 3 are applicable only for 0.30 mm≤t<3.00 mm; Mechanical properties for thicker steel strips shall be agreed upon during inquiry and ordering and cannot be directly extrapolated. Footnote a of Table 3 requires a choice between tensile indicators and hardness; Unless otherwise specified, tensile requirements apply. This page presents the alternatives separately and does not treat both as simultaneous guaranteed requirements.. For cold-rolled +CR, agree a tensile-property interval 150 MPa wide when tensile requirements are selected, or a hardness interval 50 HV wide when hardness is selected.; The outer boundaries of this table do not automatically generate actual ordering windows. Sampling, test methods, microstructure, dimensions, inspection, and other general delivery requirements shall also be verified in conjunction with EN10132-1 and applicable agreements; composition reverse-check does not replace full-item acceptance. This part applies to cold-rolled narrow steel strips for carburizing, with a standard thickness range up to 10mm; The +CR properties of 16MnCr5/17Cr3 shall be agreed upon during ordering.
Verification notes
The complete original English Table 1 was transcribed; Table 2 product-analysis tolerances and Table 3 condition/thickness and alternative tensile-or-hardness requirements have been checkedPermitted product-analysis deviations
- C
- Permitted deviation
- 0.02
- Deviation direction
- Positive or negative deviation; only one direction is permitted for the same heat
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
- Si
- Permitted deviation
- 0.03
- Deviation direction
- Only positive deviations are permitted
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
- Mn
- Permitted deviation
- 0.04
- Deviation direction
- Positive or negative deviation; only one direction is permitted for the same heat
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
- P
- Permitted deviation
- 0.005
- Deviation direction
- Only positive deviations are permitted
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
- S
- Permitted deviation
- 0.005
- Deviation direction
- Only positive deviations are permitted
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
- Cr
- Permitted deviation
- 0.03
- Deviation direction
- Positive or negative deviation; only one direction is permitted for the same heat
- Applicable conditions
- Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
C10E · DIN EN 10277:2018-09
Original table in an informative annex verified; normative composition requirements and edition still require verification. For reference only.
- Material category
- Carbon steel
- Subcategory
- Carbon steel
- Material form
- Reference record
- Composition basis
- Heat analysis in an informative annex; for reference only
- Verification status
- Original table in an informative annex verified; normative composition requirements and edition still require verification
- Standard edition
- DIN EN 10277:2018-09
- Table / clause
- Informative Annex A.3
- PDF page references
- 45
- Unit
- mass fraction (wt%)
- Analysis type
- Heat analysis (informative reference)
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.07 ~ 0.13 |
| Si | 0.15 ~ 0.4 |
| Mn | 0.3 ~ 0.6 |
| P | ≤ 0.025 (lower limit not stated) |
| S | ≤ 0.035 (lower limit not stated) |
| Cr | ≤ 0.4 (lower limit not stated) |
| Mo | ≤ 0.1 (lower limit not stated) |
| Ni | ≤ 0.4 (lower limit not stated) |
| Cu | ≤ 0.3 (lower limit not stated) |
Applicability and limitations
The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
Composition conditions
- The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
- Footnote b: A quotation is required to raise S to about 0.10% or add Pb; when S is increased, the Mn upper limit may be raised by 0.15%, but this is not automatic.
- Footnote c: Reducing Si requires other deoxidation measures.
- Unlisted elements shall not be intentionally added without the buyer’s consent.
Conditional requirement
- Footnote
- Informative boundary
- Source conditions
- The original informative annex table has been checked and is for reference only; Main-text 7.1.2 requires chemical composition to be determined under the referenced standards; the normative composition and applicable editions still require verification. It must not be used as a delivery guarantee, reverse-matching criterion or basis for carbon equivalent calculated from standard composition ranges. Main-text reference: EN ISO 683-3 (undated reference; applicable edition awaiting verification).
- Footnote
- Original-table condition 1
- Source conditions
- Footnote b: A quotation is required to raise S to about 0.10% or add Pb; when S is increased, the Mn upper limit may be raised by 0.15%, but this is not automatic.
- Footnote
- Original-table condition 2
- Source conditions
- Footnote c: Reducing Si requires other deoxidation measures.
- Footnote
- Original-table condition 3
- Source conditions
- Unlisted elements shall not be intentionally added without the buyer’s consent.