1 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
Material category
Free-cutting steel
Subcategory
Free-cutting steel
Material form
Free-cutting steel semi-finished products, bars and wire rod; see delivery-state and dimensional conditions
Original record status
Original standard verified
Standard edition
EN ISO 683-4:2018
Table / clause
Table 2 and notes a–c; Table 3; 1,6.3,7.1,7.3
PDF page references
1、5、7、10、13、14、15
Unit
Mass fraction (wt%)
Analysis type
Heat analysis
Carbon-equivalent reference
Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.
Table 2: default P≤0.11%; Default Si≤0.05%
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0300–0.1917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Table 2: default P≤0.11%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0333–0.2033 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Table 2: only as agreed in the order, P0.06–0.11%; Default Si≤0.05%
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0300–0.1917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Table 2: only as agreed in the order, P0.06–0.11%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0333–0.2033 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Table 2: only as agreed in the order, P≤0.05%; Default Si≤0.05%
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0300–0.1917 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Table 2: only as agreed in the order, P≤0.05%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
IIW / CEV:0.1000–0.3300 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.0333–0.2033 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.0600–0.2500 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Composition record (conditional branches apply; this is not an unconditional requirement)
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
≤ 0.05 (lower limit not stated)
Mn
0.6 ~ 1.2
P
≤ 0.11 (lower limit not stated)
S
0.15 ~ 0.25
Applicability and limitations
Based on the official EN ISO683-4:2018 text, consulted as DIN EN ISO683-4:2018-09; The European foreword confirms the adoption of ISO683-4:2016 without modification; 2018 is the EN adoption version year, while the adopted ISO version remains 2016. The scope includes semi-finished products, bar products, and wire rod of the free-cutting steels listed in Table 2; Bright bars shall refer separately to ISO683-18; standards for different products shall not be automatically conflated. Table 2 is for heat analysis; Verify Table 3 permissible product-analysis deviations separately only when required at ordering; deviations for the same heat must not exceed both the upper and lower limits in opposite ± directions. Grades containing Pb and grades without Pb shall be recorded separately; dashes shall not be filled as 0. The default low Si value for the non-heat-treated group shall be kept separate from the agreed Si 0.10–0.40% under special oxide guarantees; P shall be selected from a default maximum of 0.11%, an agreed range of 0.06–0.11%, or an agreed maximum of 0.05%; agreed conditions shall not be adopted automatically. Elements not listed shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking); Additions to improve machinability, such as Ca, Se, and Te, must be agreed upon and reported in the inspection documents; the complete carbon equivalent shall not be calculated based on missing items. Table 1: Untreated +U applies to semi-finished products, bar products, and wire rod; +QT delivery condition applies only to bar products listed in Table 1. Agreed properties for untreated products based on reference samples after heat treatment do not mean that wire rod has been quenched and tempered upon delivery. +U hardness in Tables 4–6 shall be kept separate from the tensile strength used for dispute arbitration; In case of dispute, determination shall be based on tensile strength; properties after quenching and tempering shall not be used to replace the untreated delivery condition. No values are listed for the first and last diameter intervals of +QT for 35SMn20/35SMnPb20 in Table 6; dashes shall not be filled as 0 or extrapolated from adjacent diameters; Parentheses for the first two hardness levels of the 44SMn28 group shall be retained as per the original text; the meaning of parentheses and the guarantee range shall be verified separately. Tensile specimens shall be according to Table 7 and ISO6892-1, with a proportional gauge length L0=5.65√S0; Sampling location, cross-section, inspection lot, and inspection document requirements shall be verified separately. According to 7.3, welding is generally not recommended for high S/P free-cutting steels; Suitability for cold heading or other cold forming must also be confirmed in conjunction with the actual material and agreement; material retrieval does not equal processing suitability or supply guarantee.
Original condition-branch records
Table 2: default P≤0.11%; Default Si≤0.05%
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
≤ 0.05 (lower limit not stated)
Mn
0.6 ~ 1.2
P
≤ 0.11 (lower limit not stated)
S
0.15 ~ 0.25
Combined limits
Subject to agreement
No
Table 2: default P≤0.11%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
0.1 ~ 0.4
Mn
0.6 ~ 1.2
P
≤ 0.11 (lower limit not stated)
S
0.15 ~ 0.25
Combined limits
Conditional requirements in the source
Footnote
Tables 2b and 2c
Source conditions
The selected P/Si exception requires an ordering agreement; the Si exception also requires guaranteed formation of the specified special oxides; Composition reverse matching does not automatically verify agreements or metallurgical evidence.
Automatic evaluation implemented
No
Subject to agreement
Yes
Table 2: only as agreed in the order, P0.06–0.11%; Default Si≤0.05%
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
≤ 0.05 (lower limit not stated)
Mn
0.6 ~ 1.2
P
0.06 ~ 0.11
S
0.15 ~ 0.25
Combined limits
Conditional requirements in the source
Footnote
Tables 2b and 2c
Source conditions
The selected P/Si exception requires an ordering agreement; the Si exception also requires guaranteed formation of the specified special oxides; Composition reverse matching does not automatically verify agreements or metallurgical evidence.
Automatic evaluation implemented
No
Subject to agreement
Yes
Table 2: only as agreed in the order, P0.06–0.11%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
0.1 ~ 0.4
Mn
0.6 ~ 1.2
P
0.06 ~ 0.11
S
0.15 ~ 0.25
Combined limits
Conditional requirements in the source
Footnote
Tables 2b and 2c
Source conditions
The selected P/Si exception requires an ordering agreement; the Si exception also requires guaranteed formation of the specified special oxides; Composition reverse matching does not automatically verify agreements or metallurgical evidence.
Automatic evaluation implemented
No
Subject to agreement
Yes
Table 2: only as agreed in the order, P≤0.05%; Default Si≤0.05%
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
≤ 0.05 (lower limit not stated)
Mn
0.6 ~ 1.2
P
≤ 0.05 (lower limit not stated)
S
0.15 ~ 0.25
Combined limits
Conditional requirements in the source
Footnote
Tables 2b and 2c
Source conditions
The selected P/Si exception requires an ordering agreement; the Si exception also requires guaranteed formation of the specified special oxides; Composition reverse matching does not automatically verify agreements or metallurgical evidence.
Automatic evaluation implemented
No
Subject to agreement
Yes
Table 2: only as agreed in the order, P≤0.05%; Si0.10–0.40% applies only by agreement and with the specified special oxides guaranteed
Element
Composition requirement
C
≤ 0.13 (lower limit not stated)
Si
0.1 ~ 0.4
Mn
0.6 ~ 1.2
P
≤ 0.05 (lower limit not stated)
S
0.15 ~ 0.25
Combined limits
Conditional requirements in the source
Footnote
Tables 2b and 2c
Source conditions
The selected P/Si exception requires an ordering agreement; the Si exception also requires guaranteed formation of the specified special oxides; Composition reverse matching does not automatically verify agreements or metallurgical evidence.
Automatic evaluation implemented
No
Subject to agreement
Yes
A condition branch must be selected
Yes
Verification notes
EN ISO683-4:2018, Table 2 and the agreed P/Si condition have been checked; The edition adopted by ISO is 2016; view properties by the selected delivery condition and diameter.
Rules for applying product-analysis deviations
Source table
Table 3
Analysis type
Product analysis only
C
Heat-analysis upper limit does not exceed
0.3
Permitted positive deviation
0.02
Permitted negative deviation
0.02
Heat-analysis upper limit greater than
0.3
Heat-analysis upper limit does not exceed
0.5
Permitted positive deviation
0.03
Permitted negative deviation
0.03
Si
Heat-analysis upper limit does not exceed
0.05
Permitted positive deviation
0.01
Permitted negative deviation
0.01
Heat-analysis upper limit greater than
0.05
Heat-analysis upper limit does not exceed
0.4
Permitted positive deviation
0.03
Permitted negative deviation
0.03
Mn
Heat-analysis upper limit does not exceed
1.0
Permitted positive deviation
0.04
Permitted negative deviation
0.04
Heat-analysis upper limit greater than
1.0
Heat-analysis upper limit does not exceed
1.7
Permitted positive deviation
0.06
Permitted negative deviation
0.06
P
Heat-analysis upper limit does not exceed
0.06
Permitted positive deviation
0.008
Permitted negative deviation
0.008
Heat-analysis upper limit greater than
0.06
Heat-analysis upper limit does not exceed
0.11
Permitted positive deviation
0.02
Permitted negative deviation
0.02
S
Heat-analysis upper limit does not exceed
0.33
Permitted positive deviation
0.03
Permitted negative deviation
0.03
Heat-analysis upper limit greater than
0.33
Heat-analysis upper limit does not exceed
0.4
Permitted positive deviation
0.04
Permitted negative deviation
0.04
Pb
Heat-analysis upper limit does not exceed
0.35
Permitted positive deviation
0.03
Permitted negative deviation
0.02
Both positive and negative deviations are permitted for the same heat