65 · GB/T 1222-2016

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Spring steels
Subcategory
Spring steels
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 1222-2016
Table / clause
Table 1 · continued table · Notes a/b; 6.1.1–6.1.3

Carbon-equivalent reference

IIW / CEV:0.7033–0.9233Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6507–0.7832Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6700–0.8137Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.62 ~ 0.7
Si0.17 ~ 0.37
Mn0.5 ~ 0.8
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.35 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)

Applicability and limitations

Heat analysis, mass fractions wt%; Product-analysis tolerances are assessed separately under GB/T222 and are not included in this table. ; Table 1, note b: when required by the purchaser and stated in the contract, residual Cu may be ≤0.20%; Default tabulated limit ≤0.25%. ; 6.1.2: oxygen in 40SiMnVBE is ≤0.0015%; oxygen in other alloy spring steels is ≤0.0025%; This limit is not extended to carbon spring steels. ; Unspecified elements do not mean zero; Spring-steel composition does not establish suitability for every cold-headed component; the specific process requires a separate assessment.

Verification notes

Table 1 and its footnotes, and the oxygen-content requirement in 6.1.2, were checked.

65 · GB /T 1222-2025

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Spring steels
Subcategory
Spring steels
Material form
Reference record
Original record status
Historical-edition reference
Standard edition
GB/T 1222-2016
Table / clause
Table 1 · continued table · Notes a/b; 6.1.1–6.1.3

Carbon-equivalent reference

IIW / CEV:0.7033–0.9233Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6507–0.7832Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6700–0.8137Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.62 ~ 0.7
Si0.17 ~ 0.37
Mn0.5 ~ 0.8
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.35 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)

Applicability and limitations

The chemical composition currently shown is transcribed from the original GB/T 1222-2016; The original record cites GB /T 1222-2025; that original edition remains unavailable, and differences between editions have not been confirmed. Heat analysis, mass fractions wt%; Product-analysis tolerances are assessed separately under GB/T222 and are not included in this table. ; Table 1, note b: when required by the purchaser and stated in the contract, residual Cu may be ≤0.20%; Default tabulated limit ≤0.25%. ; 6.1.2: oxygen in 40SiMnVBE is ≤0.0015%; oxygen in other alloy spring steels is ≤0.0025%; This limit is not extended to carbon spring steels. ; Unspecified elements do not mean zero; Spring-steel composition does not establish suitability for every cold-headed component; the specific process requires a separate assessment.

Verification notes

The chemical composition currently shown is transcribed from the original GB/T 1222-2016; The original record cites GB /T 1222-2025; that original edition remains unavailable, and differences between editions have not been confirmed.

65 · GB/T 699-1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Quality carbon structural steel (source classification)
Original record status
Original standard verified
Standard edition
GB/T 699-1999
Table / clause
Main-text Table 1, row 16, Table 2 and Clause 6.1.1
PDF page references
5、6
Unit
Mass fraction (%)
Analysis type
Ladle analysis

Carbon-equivalent reference

IIW / CEV:0.7033–0.9200Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6507–0.7823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6700–0.8125Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.62 ~ 0.7
Si0.17 ~ 0.37
Mn0.5 ~ 0.8
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

Edition 1999, main-text Table 1, row 16, unified numerical designation U20652. This record uses the default quality-steel class; heat analysis, mass fraction %. Table 2: for quality steel, P and S are each ≤0.035%; for higher-quality class A, each is ≤0.030%; for special-quality class E, the requirements are P≤0.025% and S≤0.020%. Do not apply A/E limits to the default class. 6.1.1.2—3: scrap-based steelmaking may permit Cu≤0.30%; steel for hot pressure working requires Cu≤0.20%. This record retains the default Cu≤0.25% in Table 1; specific conditions require separate confirmation. 6.1.1.4: Mn/Cr/Ni/Cu for lead-patented steel wire 35—85 has a separate restriction and does not apply to this default structural-steel record. Mechanical properties in Table 3 and 6.4 depend on specimens, dimensions, heat treatment and order requirements. Existing reference properties are not upgraded to universal guarantees by this composition review.

Verification notes

1999 original Tables 1/2 and clause 6.1.1 checked line by line.

65 · GB/T 699-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Quality carbon structural steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 699-2015
Table / clause
Table 1 and notes a and b; clauses 6.1.2 and 6.1.3

Carbon-equivalent reference

IIW / CEV:0.7033–0.9200Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6507–0.7823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6700–0.8125Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.62 ~ 0.7
Si0.17 ~ 0.37
Mn0.5 ~ 0.8
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

Table 1 of GB/T699-2015 gives heat-analysis mass fractions wt%; Product-analysis tolerances are listed separately under GB/T222. ; Table 1, note a: Cu≤0.20% for steel intended for hot pressure working; other tabulated cases are ≤0.25%. ; 6.1.2: N≤0.008% applies to basic oxygen steelmaking; analysis may be omitted if the supplier guarantees compliance; Applicability depends on the steelmaking method. ; 6.1.3: for lead-bath-patented wire, Mn0.30–0.60% for 35–85 and Mn0.70–1.00% for 65Mn/70Mn, Cr≤0.10/Ni≤0.15/Cu≤0.20%; P/S follows the corresponding wire standard and must not exceed Table 1. This is a conditional exception, not a general range. ; Elements not specified in the table must not be intentionally added without purchaser consent.

Verification notes

Table 1 and applicable clauses verified

65 · GB/T 3078-2019

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Quality carbon structural steel
Material form
Cold-drawn bars
Original record status
Original standard verified
Standard edition
GB/T 3078-2019

Carbon-equivalent reference

IIW / CEV:0.7033–0.9200Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6507–0.7823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6700–0.8125Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.62 ~ 0.7
Si0.17 ~ 0.37
Mn0.5 ~ 0.8
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

GB/T3078-2019, Clause 7.1.1: Quality carbon structural steel refers to GB/T699; alloy structural steel refers to GB/T3077.; The source of chemical composition must simultaneously display the referenced standard. ; Applies to cold-drawn steel bars and cold-drawn polished round bars.; Apply product-analysis tolerances under GB/T222 separately; do not incorporate them directly into heat-analysis ranges.. ; GB/T699-2015 Table 1: Cu≤0.20% for steel intended for hot working; this must not be mixed with the ordinary Cu≤0.25% limit.. ; For steel smelted by basic oxygen furnace, N≤0.008%; smelting method conditions must be specified. ; For grades 35–85 and 65Mn/70Mn used for lead-bath-patented wire, Mn, Cr, Ni and Cu are subject to the separate limits in Clause 6.1.3.; This record is for 3078 cold-drawn bar products, and does not automatically apply wire special cases.

Verification notes

The cited clauses in 3078 and the original texts of the referenced standards have been checked.

Hardness in the delivery condition (conditions shown separately)

GB/T 3078-2019 · Table 2 hardness in delivery condition and Note a; 7.3/7.4 · PDF pages 6, 7 · HBW

Standard condition data, not actual measured results of supplied heats; Actual delivery condition, application, and contract must be confirmed.

Cold-drawn or cold-drawn and bright-polished delivery; Table 2 conditions are for general use. For hot-pressure-working applications, check clause 7.4.2 separately.

Reference values in parentheses in the original table shall not be used as a basis for judgment: HBW ≤ 285 (lower limit not listed) HBW

Delivery in the annealed, bright-annealed, high-temperature-tempered or tempered-after-normalizing condition; delivery as-normalized is excluded and shall be agreed by both parties under 7.4.1.

HBW:≤ 255 (lower limit not stated) HBW

65 · GB /T 1222-2007

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.62 ~ 0.7
Cr≤ 0.25 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Mn0.5 ~ 0.8
Ni≤ 0.25 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Si0.17 ~ 0.37

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

65 · GB /T 13237-2013

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.62 ~ 0.7
Cr≤ 0.25 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Mn0.5 ~ 0.8
Ni≤ 0.3 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Si0.17 ~ 0.37

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

65 · GB /T 711-2017

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.62 ~ 0.7
Cr≤ 0.2 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Mn0.5 ~ 0.8
Ni≤ 0.3 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Si0.17 ~ 0.37

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

65 · GOST 14959-1979

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.62 ~ 0.7
Cr≤ 0.25 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Mn0.5 ~ 0.8
Ni≤ 0.3 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Si0.17 ~ 0.37

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

65 · YB /T 5319-2010

Original-source verification is incomplete; this is not a formal standard reference

Material category
Carbon steel
Subcategory
Carbon steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.62 ~ 0.7
Cr≤ 0.25 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Mn0.5 ~ 0.8
Ni≤ 0.25 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Si0.17 ~ 0.37

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

WhatsApp Technical enquiry →