60CrMo3-1 · DIN EN 10089-2003

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10089-2003
Table / clause
Table 3 and notes a/b and 7.1; Only the first 17 pages of the original text are available
PDF page references
1、7、9、12、13

Carbon-equivalent reference

IIW / CEV:0.8287–1.0767Known-element contribution; incomplete value; missing V, Ni; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.6340–0.7933Known-element contribution; incomplete value; missing Ni, V, B; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.6710–0.8350Known-element contribution; incomplete value; missing Ni; coupled-element constraints require separate checks; the entire envelope is not guaranteed to be realizable CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.56 ~ 0.64
Si≤ 0.4 (lower limit not stated)
Mn0.7 ~ 1.0
Cr0.7 ~ 1.0
Mo0.06 ~ 0.15
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.6 (lower limit not stated)
Sn≤ 0.06 (lower limit not stated)

Applicability and limitations

DIN EN10089:2003-04 official English original, adopting standard EN10089:2002; Table 3 heat analysis wt%. ; Cu+10Sn≤.60%; Cu≤.60/Sn≤.06 are only single-item envelopes derived from the linkage formula under the condition that each element is non-negative; they are not independent limits from the original table and the linkage formula must be satisfied simultaneously. ; Table 3 Note a: unspecified elements shall not be intentionally added without the purchaser's consent (except additions needed to finish steelmaking); blanks shall not be filled as zero. ; Note b: when hardenability is specified, C may deviate slightly but not exceed ±.01, others shall comply with Table 4 except for P/S; Default composition has not been automatically relaxed. ; This document contains only the first 17 pages; Table 3 is complete and verifiable; Hardenability Tables 7/8 and other missing pages need to be supplemented separately; the completeness of the entire standard is not claimed. ; Hot-rolled spring steels intended for quenching and tempering; composition or annealed condition alone does not establish cold-heading suitability or actual supply..

Combined limits

Combined-element limits
  • Element coefficient
    Cu
    1
    Sn
    10
    Upper limit
    0.6
    Requirement
    Cu + 10Sn ≤ 0.60 wt%

Verification notes

Official original Table 3: all 19 rows and footnotes visually checked.

Jominy end-quench hardenability (conditional requirements)

EN 10089:2002 · BS EN 10089:2002 · Tables 7/8, 7.1.2–7.1.4 and Table 10 · PDF pages 6, 9, 17, 18, 20, 21

+H normal hardenability band (7.1.2)

End-quench test condition temperature 850 ± 5 °C; This is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.55766
35766
55766
75665
95665
115665
135465
155364
205064
254363
303663
353262
403062
453061
503060

+HH restricted hardenability band (7.1.4)

End-quench test condition temperature 850 ± 5 °C; This is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.56066
36066
56066
75965
95965
115965
135865
155764
205564
255063
304563
354262
404162
454061
504060
WhatsApp Technical enquiry →