← BackMaterial grade directory

36SMN14

3 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 36SMN14 →

36SMn14 · EN ISO 683-4-2018

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Free-cutting steel
Subcategory
Free-cutting steel
Material form
Free-cutting steel semi-finished products, bars and wire rod; see delivery-state and dimensional conditions
Original record status
Original standard verified
Standard edition
EN ISO 683-4:2018
Table / clause
Table 2 and notes a–c; Table 3; 1,6.3,7.1,7.3
PDF page references
1、5、7、10、13、14、15
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.5367–0.6733 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4883 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4500–0.5600 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si≤ 0.4 (lower limit not stated)
Mn1.3 ~ 1.7
P≤ 0.06 (lower limit not stated)
S0.1 ~ 0.18

Applicability and limitations

Based on the official EN ISO683-4:2018 text, consulted as DIN EN ISO683-4:2018-09; The European foreword confirms the adoption of ISO683-4:2016 without modification; 2018 is the EN adoption version year, while the adopted ISO version remains 2016. The scope includes semi-finished products, bar products, and wire rod of the free-cutting steels listed in Table 2; Bright bars shall refer separately to ISO683-18; standards for different products shall not be automatically conflated. Table 2 is for heat analysis; Verify Table 3 permissible product-analysis deviations separately only when required at ordering; deviations for the same heat must not exceed both the upper and lower limits in opposite ± directions. Grades containing Pb and grades without Pb shall be recorded separately; dashes shall not be filled as 0. The default low Si value for the non-heat-treated group shall be kept separate from the agreed Si 0.10–0.40% under special oxide guarantees; P shall be selected from a default maximum of 0.11%, an agreed range of 0.06–0.11%, or an agreed maximum of 0.05%; agreed conditions shall not be adopted automatically. Elements not listed shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking); Additions to improve machinability, such as Ca, Se, and Te, must be agreed upon and reported in the inspection documents; the complete carbon equivalent shall not be calculated based on missing items. Table 1: Untreated +U applies to semi-finished products, bar products, and wire rod; +QT delivery condition applies only to bar products listed in Table 1. Agreed properties for untreated products based on reference samples after heat treatment do not mean that wire rod has been quenched and tempered upon delivery. +U hardness in Tables 4–6 shall be kept separate from the tensile strength used for dispute arbitration; In case of dispute, determination shall be based on tensile strength; properties after quenching and tempering shall not be used to replace the untreated delivery condition. No values are listed for the first and last diameter intervals of +QT for 35SMn20/35SMnPb20 in Table 6; dashes shall not be filled as 0 or extrapolated from adjacent diameters; Parentheses for the first two hardness levels of the 44SMn28 group shall be retained as per the original text; the meaning of parentheses and the guarantee range shall be verified separately. Tensile specimens shall be according to Table 7 and ISO6892-1, with a proportional gauge length L0=5.65√S0; Sampling location, cross-section, inspection lot, and inspection document requirements shall be verified separately. According to 7.3, welding is generally not recommended for high S/P free-cutting steels; Suitability for cold heading or other cold forming must also be confirmed in conjunction with the actual material and agreement; material retrieval does not equal processing suitability or supply guarantee.

Verification notes

EN ISO683-4:2018, Table 2 and the agreed P/Si condition have been checked; The edition adopted by ISO is 2016; view properties by the selected delivery condition and diameter.

Rules for applying product-analysis deviations

Source table
Table 3
Analysis type
Product analysis only
C
  • Heat-analysis upper limit does not exceed
    0.3
    Permitted positive deviation
    0.02
    Permitted negative deviation
    0.02
  • Heat-analysis upper limit greater than
    0.3
    Heat-analysis upper limit does not exceed
    0.5
    Permitted positive deviation
    0.03
    Permitted negative deviation
    0.03
Si
  • Heat-analysis upper limit does not exceed
    0.05
    Permitted positive deviation
    0.01
    Permitted negative deviation
    0.01
  • Heat-analysis upper limit greater than
    0.05
    Heat-analysis upper limit does not exceed
    0.4
    Permitted positive deviation
    0.03
    Permitted negative deviation
    0.03
Mn
  • Heat-analysis upper limit does not exceed
    1.0
    Permitted positive deviation
    0.04
    Permitted negative deviation
    0.04
  • Heat-analysis upper limit greater than
    1.0
    Heat-analysis upper limit does not exceed
    1.7
    Permitted positive deviation
    0.06
    Permitted negative deviation
    0.06
P
  • Heat-analysis upper limit does not exceed
    0.06
    Permitted positive deviation
    0.008
    Permitted negative deviation
    0.008
  • Heat-analysis upper limit greater than
    0.06
    Heat-analysis upper limit does not exceed
    0.11
    Permitted positive deviation
    0.02
    Permitted negative deviation
    0.02
S
  • Heat-analysis upper limit does not exceed
    0.33
    Permitted positive deviation
    0.03
    Permitted negative deviation
    0.03
  • Heat-analysis upper limit greater than
    0.33
    Heat-analysis upper limit does not exceed
    0.4
    Permitted positive deviation
    0.04
    Permitted negative deviation
    0.04
Pb
  • Heat-analysis upper limit does not exceed
    0.35
    Permitted positive deviation
    0.03
    Permitted negative deviation
    0.02
Both positive and negative deviations are permitted for the same heat
No
Used to relax heat-analysis requirements
No

36SMn14 · EN 10087-1998

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Free-cutting steel
Material form
Free-cutting steel semi-finished products, bars and wire rod; delivery state according to the standard and order
Original record status
Original standard verified
Standard edition
EN 10087:1998
Table / clause
Table 1 and footnote a/b
PDF page references
1、6
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.5367–0.6733 Known-item contribution, not a complete value; missing Cr, Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3850–0.4883 Known-item contribution, not a complete value; missing Cu, Cr, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4500–0.5600 Known-item contribution, not a complete value; missing Mo, Cr, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si≤ 0.4 (lower limit not stated)
Mn1.3 ~ 1.7
P≤ 0.06 (lower limit not stated)
S0.1 ~ 0.18

Applicability and limitations

Original 1998 edition Table 1 gives cast analysis in mass percent wt%; unlisted elements are not zero.

Permissible product-analysis deviations in Table 2 cannot be added to Table 1 cast-analysis limits.

This standard covers free-cutting steel bars, wire rod and semi-finished products; specific delivery/heat treatment and cold-heading suitability require separate verification.

Verification notes

EN 10087:1998 scanned original, Table 1, row 10 visually checked; independent of EN ISO 683-4:2018.

Mechanical-property conditions selected by size and delivery condition

EN10087:1998 · Tables 3–5 and footnotes, 6.2, 8.2.1.1, Table 8, B.1/B.4; Guideline values in Tables 6/7 are not process recommendations · PDF pages 4, 5, 7, 8, 9, 10, 12

Applicable conditionsTensile strength Rm(N/mm²)Yield strength Re(source table: 0.2% proof stress;N/mm²)Elongation after fracture A(%;L₀=5d₀)Brinell hardness HB(reference only; not an independent acceptance guarantee)
Untreated condition · 5 ≤ d ≤ 10 mm580 ~ 770Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0
Quenched-and-tempered delivery (must be adopted in the order) · 5 ≤ d ≤ 10 mm700 ~ 850≥ 480 (upper limit not stated)≥ 14 (upper limit not stated)Not listed in the original table or not applicable to this condition; do not substitute 0
Untreated condition · 10 < d ≤ 16 mm580 ~ 770Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0
Quenched and tempered delivery (must be specified in the order) · 10 < d ≤ 16 mm700 ~ 850≥ 460 (upper limit not stated)≥ 14 (upper limit not stated)Not listed in the original table or not applicable to this condition; do not substitute 0
Untreated condition · 16 < d ≤ 40 mm560 ~ 750Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0166 ~ 222
Quenched and tempered delivery (must be specified in the order) · 16 < d ≤ 40 mm670 ~ 820≥ 420 (upper limit not stated)≥ 15 (upper limit not stated)Not listed in the original table or not applicable to this condition; do not substitute 0
Untreated condition · 40 < d ≤ 63 mm560 ~ 740Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0166 ~ 219
Quenched and tempered delivery (must be specified in the order) · 40 < d ≤ 63 mm640 ~ 790≥ 400 (upper limit not stated)≥ 16 (upper limit not stated)Not listed in the original table or not applicable to this condition; do not substitute 0
Untreated condition · 63 < d ≤ 100 mm550 ~ 740Not listed in the original table or not applicable to this condition; do not substitute 0Not listed in the original table or not applicable to this condition; do not substitute 0163 ~ 219
Quenched and tempered delivery (must be specified in the order) · 63 < d ≤ 100 mm570 ~ 720≥ 360 (upper limit not stated)≥ 17 (upper limit not stated)Not listed in the original table or not applicable to this condition; do not substitute 0

Welding limitations in the source standard

Due to higher sulfur and phosphorus content, free-cutting steels in this standard are generally not recommended for welding. Carbon equivalent calculation results do not constitute approval for weldability, welding processes, or material substitution.

EN10087:1998 · 7.2 · PDF page 4

Permitted product-analysis deviations (must not be added to heat-analysis limits)

EN10087:1998 · Table 2 and Note a, B.4 · PDF pages 6, 12 · mass fraction wt%; Deviations are expressed in percentage points of mass percentage

Product analysis only; does not modify heat composition or automatic calculation/matching boundaries. Applicable entries exist only for elements specified in the original table.

ElementSpecified maximum heat-analysis content, wt%Lower deviation, percentage pointsUpper deviation, percentage pointsApplicable conditions
CSpecified maximum content ≤ 0.3-0.02+0.02Select the band for the specified maximum content in the original table
C0.3 < specified maximum content ≤ 0.5-0.03+0.03Select the band for the specified maximum content in the original table
SiSpecified maximum content ≤ 0.05The original table does not state a negative deviation+0.01Select the band for the specified maximum content in the original table
Si0.05 < specified maximum content ≤ 0.4The original table does not state a negative deviation+0.03Select the band for the specified maximum content in the original table
MnSpecified maximum content ≤ 1-0.04+0.04Select the band for the specified maximum content in the original table
Mn1 < specified maximum content ≤ 1.7-0.06+0.06Select the band for the specified maximum content in the original table
PSpecified maximum content ≤ 0.06The original table does not state a negative deviation+0.008Select the band for the specified maximum content in the original table
P0.06 < specified maximum content ≤ 0.11The original table does not state a negative deviation+0.02Select the band for the specified maximum content in the original table
SSpecified maximum content ≤ 0.33-0.03+0.03Select the band for the specified maximum content in the original table
S0.33 < specified maximum content ≤ 0.4-0.04+0.04Select the band for the specified maximum content in the original table
PbSpecified maximum content ≤ 0.35-0.02+0.03Select the band for the specified maximum content in the original table

This is a complete standard deviation table and does not imply that every element for this grade is specified; Elements not listed are not added on the basis of this table. Symmetric deviation for the same heat is permitted in only one direction, either upward or downward; Asymmetric deviation for Pb is only found in the Pb row of EN10087 and cannot be applied to other standards where Pb is not listed. Do not automatically expand heat analysis composition, carbon equivalent, or reverse-lookup ranges.

36SMn14 · DIN EN 10277:2018-09

Original table in an informative annex verified; normative composition requirements and edition still require verification. For reference only.

Material category
Carbon steel
Subcategory
Free-cutting steel
Material form
Reference record
Composition basis
Heat analysis in an informative annex; for reference only
Verification status
Original table in an informative annex verified; normative composition requirements and edition still require verification
Standard edition
DIN EN 10277:2018-09
Table / clause
Informative Annex A.2
PDF page references
44
Unit
mass fraction (wt%)
Analysis type
Heat analysis (informative reference)

Carbon-equivalent reference

Composition from an informative standard annex is for reference only. Normative composition and edition remain unverified; standard-range carbon equivalents and reverse matching are disabled.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si≤ 0.4 (lower limit not stated)
Mn1.3 ~ 1.7
P≤ 0.06 (lower limit not stated)
S0.1 ~ 0.18

Applicability and limitations

The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.

Composition conditions

Conditional requirement

Verification notes

The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
WhatsApp Technical enquiry →