35SMN20
2 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for 35SMN20 →35SMn20 · EN ISO 683-4-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material category
- Free-cutting steel
- Subcategory
- Free-cutting steel
- Material form
- Free-cutting steel semi-finished products, bars and wire rod; see delivery-state and dimensional conditions
- Original record status
- Original standard verified
- Standard edition
- EN ISO 683-4:2018
- Table / clause
- Table 2 and notes a–c; Table 3; 1,6.3,7.1,7.3
- PDF page references
- 1、5、7、10、13、14、15
- Unit
- Mass fraction (wt%)
- Analysis type
- Heat analysis
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.32 ~ 0.39 |
| Si | ≤ 0.4 (lower limit not stated) |
| Mn | 0.9 ~ 1.4 |
| P | ≤ 0.06 (lower limit not stated) |
| S | 0.15 ~ 0.25 |
Applicability and limitations
Based on the official EN ISO683-4:2018 text, consulted as DIN EN ISO683-4:2018-09; The European foreword confirms the adoption of ISO683-4:2016 without modification; 2018 is the EN adoption version year, while the adopted ISO version remains 2016. The scope includes semi-finished products, bar products, and wire rod of the free-cutting steels listed in Table 2; Bright bars shall refer separately to ISO683-18; standards for different products shall not be automatically conflated. Table 2 is for heat analysis; Verify Table 3 permissible product-analysis deviations separately only when required at ordering; deviations for the same heat must not exceed both the upper and lower limits in opposite ± directions. Grades containing Pb and grades without Pb shall be recorded separately; dashes shall not be filled as 0. The default low Si value for the non-heat-treated group shall be kept separate from the agreed Si 0.10–0.40% under special oxide guarantees; P shall be selected from a default maximum of 0.11%, an agreed range of 0.06–0.11%, or an agreed maximum of 0.05%; agreed conditions shall not be adopted automatically. Elements not listed shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking); Additions to improve machinability, such as Ca, Se, and Te, must be agreed upon and reported in the inspection documents; the complete carbon equivalent shall not be calculated based on missing items. Table 1: Untreated +U applies to semi-finished products, bar products, and wire rod; +QT delivery condition applies only to bar products listed in Table 1. Agreed properties for untreated products based on reference samples after heat treatment do not mean that wire rod has been quenched and tempered upon delivery. +U hardness in Tables 4–6 shall be kept separate from the tensile strength used for dispute arbitration; In case of dispute, determination shall be based on tensile strength; properties after quenching and tempering shall not be used to replace the untreated delivery condition. No values are listed for the first and last diameter intervals of +QT for 35SMn20/35SMnPb20 in Table 6; dashes shall not be filled as 0 or extrapolated from adjacent diameters; Parentheses for the first two hardness levels of the 44SMn28 group shall be retained as per the original text; the meaning of parentheses and the guarantee range shall be verified separately. Tensile specimens shall be according to Table 7 and ISO6892-1, with a proportional gauge length L0=5.65√S0; Sampling location, cross-section, inspection lot, and inspection document requirements shall be verified separately. According to 7.3, welding is generally not recommended for high S/P free-cutting steels; Suitability for cold heading or other cold forming must also be confirmed in conjunction with the actual material and agreement; material retrieval does not equal processing suitability or supply guarantee.
Verification notes
EN ISO683-4:2018, Table 2 and the agreed P/Si condition have been checked; The edition adopted by ISO is 2016; view properties by the selected delivery condition and diameter.Rules for applying product-analysis deviations
- Source table
- Table 3
- Analysis type
- Product analysis only
- C
- Heat-analysis upper limit does not exceed
- 0.3
- Permitted positive deviation
- 0.02
- Permitted negative deviation
- 0.02
- Heat-analysis upper limit greater than
- 0.3
- Heat-analysis upper limit does not exceed
- 0.5
- Permitted positive deviation
- 0.03
- Permitted negative deviation
- 0.03
- Si
- Heat-analysis upper limit does not exceed
- 0.05
- Permitted positive deviation
- 0.01
- Permitted negative deviation
- 0.01
- Heat-analysis upper limit greater than
- 0.05
- Heat-analysis upper limit does not exceed
- 0.4
- Permitted positive deviation
- 0.03
- Permitted negative deviation
- 0.03
- Mn
- Heat-analysis upper limit does not exceed
- 1.0
- Permitted positive deviation
- 0.04
- Permitted negative deviation
- 0.04
- Heat-analysis upper limit greater than
- 1.0
- Heat-analysis upper limit does not exceed
- 1.7
- Permitted positive deviation
- 0.06
- Permitted negative deviation
- 0.06
- P
- Heat-analysis upper limit does not exceed
- 0.06
- Permitted positive deviation
- 0.008
- Permitted negative deviation
- 0.008
- Heat-analysis upper limit greater than
- 0.06
- Heat-analysis upper limit does not exceed
- 0.11
- Permitted positive deviation
- 0.02
- Permitted negative deviation
- 0.02
- S
- Heat-analysis upper limit does not exceed
- 0.33
- Permitted positive deviation
- 0.03
- Permitted negative deviation
- 0.03
- Heat-analysis upper limit greater than
- 0.33
- Heat-analysis upper limit does not exceed
- 0.4
- Permitted positive deviation
- 0.04
- Permitted negative deviation
- 0.04
- Pb
- Heat-analysis upper limit does not exceed
- 0.35
- Permitted positive deviation
- 0.03
- Permitted negative deviation
- 0.02
- Both positive and negative deviations are permitted for the same heat
- No
- Used to relax heat-analysis requirements
- No
35SMn20 · DIN EN 10277:2018-09
Original table in an informative annex verified; normative composition requirements and edition still require verification. For reference only.
- Material category
- Carbon steel
- Subcategory
- Free-cutting steel
- Material form
- Reference record
- Composition basis
- Heat analysis in an informative annex; for reference only
- Verification status
- Original table in an informative annex verified; normative composition requirements and edition still require verification
- Standard edition
- DIN EN 10277:2018-09
- Table / clause
- Informative Annex A.2
- PDF page references
- 44
- Unit
- mass fraction (wt%)
- Analysis type
- Heat analysis (informative reference)
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.32 ~ 0.39 |
| Si | ≤ 0.4 (lower limit not stated) |
| Mn | 0.9 ~ 1.4 |
| P | ≤ 0.06 (lower limit not stated) |
| S | 0.15 ~ 0.25 |
Applicability and limitations
The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
Composition conditions
- The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
- Unlisted elements must not be intentionally added without purchaser consent; Machinability-improving additions such as Ca/Se/Te require agreement and must be stated in the certificate.
- Footnote b: Si 0.10—0.40% is an agreed option for specific oxide control and does not replace the default Si maximum.
- Footnote c: P 0.06—0.11% or ≤0.05% requires agreement at enquiry or ordering; Default original-table values are not rewritten automatically.
Conditional requirement
- Footnote
- Informative boundary
- Source conditions
- The original informative annex table has been checked and is for reference only; Main-text 7.1.2 requires chemical composition to be determined under the referenced standards; the normative composition and applicable editions still require verification. It must not be used as a delivery guarantee, reverse-matching criterion or basis for carbon equivalent calculated from standard composition ranges. Main-text reference: EN ISO 683-4 (undated reference; applicable edition awaiting verification).
- Footnote
- Original-table condition 1
- Source conditions
- Unlisted elements must not be intentionally added without purchaser consent; Machinability-improving additions such as Ca/Se/Te require agreement and must be stated in the certificate.
- Footnote
- Original-table condition 2
- Source conditions
- Footnote b: Si 0.10—0.40% is an agreed option for specific oxide control and does not replace the default Si maximum.
- Footnote
- Original-table condition 3
- Source conditions
- Footnote c: P 0.06—0.11% or ≤0.05% requires agreement at enquiry or ordering; Default original-table values are not rewritten automatically.