← BackMaterial grade directory

35MN

3 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 35MN →

35Mn · GB/T 699-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Quality carbon structural steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 699-2015
Table / clause
Table 1 and notes a and b; clauses 6.1.2 and 6.1.3

Carbon-equivalent reference

IIW / CEV:0.4367–0.6433Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3607–0.4823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3900–0.5225Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si0.17 ~ 0.37
Mn0.7 ~ 1.0
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

Table 1 of GB/T699-2015 gives heat-analysis mass fractions wt%; Product-analysis tolerances are listed separately under GB/T222. ; Table 1, note a: Cu≤0.20% for steel intended for hot pressure working; other tabulated cases are ≤0.25%. ; 6.1.2: N≤0.008% applies to basic oxygen steelmaking; analysis may be omitted if the supplier guarantees compliance; Applicability depends on the steelmaking method. ; 6.1.3: for lead-bath-patented wire, Mn0.30–0.60% for 35–85 and Mn0.70–1.00% for 65Mn/70Mn, Cr≤0.10/Ni≤0.15/Cu≤0.20%; P/S follows the corresponding wire standard and must not exceed Table 1. This is a conditional exception, not a general range. ; Elements not specified in the table must not be intentionally added without purchaser consent.

Verification notes

Table 1 and applicable clauses verified

35Mn · GB/T 699-1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Material form
Quality carbon structural steel (source classification)
Original record status
Original standard verified
Standard edition
GB/T 699-1999
Table / clause
Main-text Table 1, row 25, Table 2 and Clause 6.1.1
PDF page references
5、6
Unit
Mass fraction (%)
Analysis type
Ladle analysis

Carbon-equivalent reference

IIW / CEV:0.4367–0.6433Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3607–0.4823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3900–0.5225Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si0.17 ~ 0.37
Mn0.7 ~ 1.0
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)

Applicability and limitations

Edition 1999, main-text Table 1, row 25, unified numerical designation U21352. This record uses the default quality-steel class; heat analysis, mass fraction %. Table 2: for quality steel, P and S are each ≤0.035%; for higher-quality class A, each is ≤0.030%; for special-quality class E, the requirements are P≤0.025% and S≤0.020%. Do not apply A/E limits to the default class. 6.1.1.2—3: scrap-based steelmaking may permit Cu≤0.30%; steel for hot pressure working requires Cu≤0.20%. This record retains the default Cu≤0.25% in Table 1; specific conditions require separate confirmation. 6.1.1.4: Mn/Cr/Ni/Cu for lead-patented steel wire 35—85 has a separate restriction and does not apply to this default structural-steel record. Mechanical properties in Table 3 and 6.4 depend on specimens, dimensions, heat treatment and order requirements. Existing reference properties are not upgraded to universal guarantees by this composition review.

Verification notes

1999 original Tables 1/2 and clause 6.1.1 checked line by line.

35Mn · GB/T 3078-2019

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Carbon steel
Subcategory
Quality carbon structural steel
Material form
Cold-drawn bars
Original record status
Original standard verified
Standard edition
GB/T 3078-2019

Carbon-equivalent reference

IIW / CEV:0.4367–0.6433Known-element contribution; incomplete value; missing Mo, V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3607–0.4823Known-element contribution; incomplete value; missing Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3900–0.5225Known-element contribution; incomplete value; missing Mo CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.32 ~ 0.39
Si0.17 ~ 0.37
Mn0.7 ~ 1.0
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr≤ 0.25 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

Clause 7.1.1 of GB/T3078—2019: quality carbon structural steel follows GB/T699, and alloy structural steel follows GB/T3077; The referenced composition standard must also be shown. This grade is listed in Table 2, row 17; Hardness by delivery condition is listed under separate conditions in Table 2; Actual use and delivery condition require separate verification and are not automatically treated as satisfied. Cold-drawn steel bars

cold-drawn polished round steel; Product-analysis tolerances under GB/T222 require separate verification and are not added to the heat-analysis range. Table 1 of GB/T699-2015 gives heat-analysis mass fractions wt%; Product-analysis tolerances are listed separately under GB/T222. Table 1, note a: Cu≤0.20% for steel intended for hot pressure working; other tabulated cases are ≤0.25%. 6.1.2: N≤0.008% applies to basic oxygen steelmaking; analysis may be omitted if the supplier guarantees compliance; Applicability depends on the steelmaking method. 6.1.3: for lead-bath-patented wire, Mn0.30–0.60% for 35–85 and Mn0.70–1.00% for 65Mn/70Mn, Cr≤0.10/Ni≤0.15/Cu≤0.20%; P/S follows the corresponding wire standard and must not exceed Table 1. This is a conditional exception, not a general range. Elements not specified in the table must not be intentionally added without purchaser consent.

Verification notes

The grade row in GB/T3078—2019, Table 2 and the 7.1.1 reference clause have been checked; Composition comes from verified original GB/T 699-2015, not a separate GB/T3078 composition table

Hardness in the delivery condition (conditions shown separately)

GB/T 3078-2019 · Table 2 hardness in delivery condition and Note a; 7.3/7.4 · PDF pages 6, 7 · HBW

Standard condition data, not actual measured results of supplied heats; Actual delivery condition, application, and contract must be confirmed.

Cold-drawn or cold-drawn and bright-polished delivery; Table 2 conditions are for general use. For hot-pressure-working applications, check clause 7.4.2 separately.

HBW:≤ 255 (lower limit not stated) HBW

Delivery in the annealed, bright-annealed, high-temperature-tempered or tempered-after-normalizing condition; delivery as-normalized is excluded and shall be agreed by both parties under 7.4.1.

HBW:≤ 207 (lower limit not stated) HBW

WhatsApp Technical enquiry →