← BackMaterial grade directory

30MNVS6

5 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 30MNVS6 →

30MnVS6 · Q/BQB 517-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Cold-heading steel
Material form
Hot-rolled steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
Q/BQB 517—2023
Table / clause
6.1.1/Table 1, row 100, note a
PDF page references
12
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Source document

Original composition-element notation and analysis basis
Al
Original element symbol
Alₜ
Symbol extracted from the original source
Alt
Original table column heading
Al t
Subscript in the original source
t
Subscript explanation
Only original table subscripts shall be retained; do not expand these into total aluminum or acid-soluble aluminum; Al without specified form shall not be directly equated
Standard edition
Q/BQB 517—2023
Table / clause
1
Original table item number
100
PDF page references
12
Unit
Mass fraction (wt%)
Analysis type
Heat analysis
Original record status
Original column symbol verified
Original cell
0.010 ~ 0.025

When the original analysis designations differ, or a record leaves them unspecified, comparability or a match cannot be concluded directly. Subscripts not explained by the source are not expanded here.

Carbon-equivalent reference

IIW / CEV:0.5067–0.6460 Independent-element envelope of standard ranges; not measured heat-analysis values CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3633–0.4447Known-element contribution; incomplete value; missing B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.4000–0.4812 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.27 ~ 0.31
Si0.55 ~ 0.7
Mn1.3 ~ 1.4
P≤ 0.015 (lower limit not stated)
S0.012 ~ 0.025
Mo≤ 0.05 (lower limit not stated)
Alₜ0.01 ~ 0.025
V0.1 ~ 0.13
Ni≤ 0.15 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
N0.01 ~ 0.02
Cr≤ 0.2 (lower limit not stated)

Applicability and limitations

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 100; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Verification notes

All 104 rows of Table 1 and 34 rows of Table 2 in the original Q/BQB517:2023 from Baosteel’s official website were checked row by row; not mixed with older editions.View associated products →

30MnVS6 · EN 10267-1998

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Precipitation-hardening ferritic-pearlitic steel
Material form
Semi-finished products and bars for hot working; select delivery condition +U, +S or +P and verify against Table 1
Original record status
Original standard verified
Standard edition
EN 10267:1998
Table / clause
Table 3 and footnotes 1–4; Table 1 applicability
PDF page references
1、7、9
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Carbon-equivalent reference

IIW / CEV:0.4760–0.7127Known-element contribution; incomplete value; missing Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3330–0.4770Known-element contribution; incomplete value; missing Cu, Ni, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3800–0.5130Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.26 ~ 0.33
Si0.15 ~ 0.8
Mn1.2 ~ 1.6
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.06
N0.01 ~ 0.02
Cr≤ 0.3 (lower limit not stated)
Mo≤ 0.08 (lower limit not stated)
V0.08 ~ 0.2

Applicability and limitations

Table 3 of EN 10267:1998 is heat analysis mass fraction wt%. ; Table 1: Table 3 and Table 4 are used for untreated +U and cold-sheared +S deliveries; The chemical composition in Table 5 for precipitation hardening +P machined bars is for guidance only; Table 3 shall not be automatically regarded as a +P delivery guarantee. ; Table 3 Footnote 2: Other elements for improving machinability or controlling sulfides/oxides, as well as adjustments to the sulfur range, shall be by agreement. ; Table 3 Footnote 3: Partial or total substitution of V by Nb requires agreement; the lower limit of V must also be separately negotiated; Current composition reverse-checks shall only use the default limits of Table 3 without substitutions. ; Table 3 Footnote 4: Ti addition shall be by agreement; Elements not listed shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking). ; Product analysis deviations in Table 4 shall be verified separately; The +P mechanical properties in Table 5 correspond only to machined bars and 30–120mm; other sizes shall be by agreement; Cold-heading suitability shall be verified separately.

Verification notes

EN 10267:1998, Table 3, row 2, and Table 1 / footnotes were checked item by item; Composition in the +P condition is for guidance only.

30MnVS6 · Q/XG 243-2019

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Material form
Wire rod
Original record status
Original standard verified
Standard edition
Q/XG 243-2019
Table / clause
Table 3, row 10
PDF page references
3
Unit
Mass fraction (wt%)

Carbon-equivalent reference

IIW / CEV:0.5110–0.6993 Independent-element envelope of standard ranges; not measured heat-analysis values CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3472–0.4645Known-element contribution; incomplete value; missing B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3900–0.5068 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.25 ~ 0.31
Si0.5 ~ 0.8
Mn1.35 ~ 1.6
P≤ 0.025 (lower limit not stated)
S0.01 ~ 0.04
Cr0.1 ~ 0.25
Mo≤ 0.08 (lower limit not stated)
V0.08 ~ 0.15
N0.01 ~ 0.025
Al≤ 0.025 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Ni≤ 0.15 (lower limit not stated)

Applicability and limitations

Mass fraction wt%; Q/XG 243-2019 heat analysis; Local PDF, page 3. Check product-analysis tolerances under GB/T 222; Heat-analysis ranges are not directly treated as guaranteed product-analysis ranges. The enterprise standard covers passenger-vehicle cold-heading steel wire rod requiring vehicle-manufacturer approval; it does not establish Creation Group stock availability, customer approval or substitution approval.

Combined limits

Combined-element limits
    Elements requiring measured values from the same heat

      Verification notes

      Original Q/XG 243-2019, Table 3 PDF, page 3: rows and merged cells were visually checked

      30MnVS6 · BEXG 021-2020

      Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

      Material category
      Cold-heading steel
      Subcategory
      Cold-heading steel
      Material form
      Wire rod
      Original record status
      Manufacturer source verified
      Document edition
      BEXG 021-2020, sixteenth revision stated on the cover; issued and effective on 2020-12-29; The latest original document available on this computer only
      Document title
      Technical delivery conditions for cold-heading steel wire rod for automotive parts
      Table / clause
      Table 1
      PDF page references
      5
      Unit
      Mass fraction (wt%)
      Manufacturer
      Baoshan Iron & Steel Co., Ltd. (Baosteel)

      Carbon-equivalent reference

      Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

      IIW / CEV:0.5307–0.6460 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
      Pcm(Ito–Bessyo):0.3693–0.4447Known-element contribution; incomplete value; missing B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
      CET:0.4060–0.4812 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

      Composition

      ElementComposition requirement
      C0.27 ~ 0.31
      Si0.55 ~ 0.7
      Mn1.3 ~ 1.4
      P≤ 0.015 (lower limit not stated)
      S0.012 ~ 0.025
      Cr0.12 ~ 0.2
      Ni≤ 0.15 (lower limit not stated)
      Cu≤ 0.25 (lower limit not stated)
      Al0.01 ~ 0.025
      Mo≤ 0.05 (lower limit not stated)
      V0.1 ~ 0.13
      N0.01 ~ 0.02

      Applicability and limitations

      Baosteel BEXG 021-2020, Table 1, row 29, PDF page 5; heat-analysis composition in wt%, hot-rolled wire rod. 2020 is the original edition available locally, with no claim that it is the company’s current latest edition. Special conditions and actual supply require separate confirmation.

      Composition conditions

      Verification notes

      Table 1 original images checked page by page, physical pages 3–10; continuation values and other columns kept separate; two disputed rows excluded.

      Source footnotes

      Ni:≤0.15;Cu:≤0.25;Al:0.010-0.025;Mo:≤0.05;V:0.10-0.13;N:0.010-0.020View associated products →

      30MnVS6 · Ovako Product Catalogue CO-117 ENG 24:07 (2024)

      Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

      Material category
      Carbon steel
      Subcategory
      Carbon steel
      Material form
      Bars, tubes, rings and precomponents
      Composition basis
      Manufacturer typical/nominal values, not guaranteed ranges
      Original record status
      Manufacturer source verified
      Document edition
      CO-117 ENG 24:07 ©Ovako 2024
      Document title
      Ovako Product Catalogue
      PDF page references
      44
      Unit
      Interpreted as mass fraction (%) using other documents from the same manufacturer; the unit is not explicitly stated in this table
      Analysis type
      Typical composition analysis
      Manufacturer
      Ovako

      Source document

      Carbon-equivalent reference

      Manufacturer typical single values are composition references only; no range estimate is made. They are neither standard guarantees nor measured heat results; Formula applicability requires review against the intended use and process.

      IIW / CEV: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
      Pcm (Ito–Bessyo): manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
      CET: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated

      Composition

      ElementComposition requirement
      CTypical/nominal value 0.3 (not a guaranteed range)
      SiTypical/nominal value 0.5 (not a guaranteed range)
      MnTypical/nominal value 1.4 (not a guaranteed range)

      Applicability and limitations

      Ovako 2024 product catalogue, PDF page 44; manufacturer’s typical analysis, for composition reference only. The original header does not explicitly state units; interpreted using the manufacturer’s mass-fraction % information. Neither standard guaranteed values nor measured heat analysis. Excluded from limit-based reverse search and carbon-equivalent calculation; blanks and element names alone in the other-elements field are not filled with 0. Manufacturer code: 9830.

      Conditional requirement

      Verification notes

      All 170 rows of the 2021 original table were visually checked. Values in corresponding 2024 cells are unchanged; recognition differences were reviewed separately. Rows with conflicting values under the same code are excluded; values are not mixed across sections.

      Source notes

      Micro-alloyed cold heading steel. Used for short- and long-shaft ball points, threaded and heavy duty anchor bolts

      Other-element requirements

      V
      WhatsApp Technical enquiry →