28CRS4

7 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 28CRS4 →

28CrS4 · DIN 17200-1987

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN 17200-1987-03
Table / clause
Table 2 and footnotes 1–5; 7.3.1–7.3.2
PDF page references
1、2、15、16、17

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.4283Known-element contribution; incomplete value; missing Cu, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3450–0.4600Known-element contribution; incomplete value; missing Mo, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.24 ~ 0.31
Mn0.6 ~ 0.9
S0.02 ~ 0.035
Cr0.9 ~ 1.2
Si≤ 0.4 (lower limit not stated)
P≤ 0.035 (lower limit not stated)

Applicability and limitations

Table 2 cast analysis, mass fraction wt%; Si is an upper limit and unspecified elements are not filled with zero. P/S requirements for the C, Ck and Cm series remain separate; S 0.020–0.035% in S-containing grades is a two-sided range. Note 1: unlisted elements may not be intentionally added without purchaser consent, except to complete melting; no fixed residual values are inferred. Table 3 contains permissible product-analysis deviations, not added to cast limits; applicable sizes and positive/negative directions are checked separately. Heat-treatment condition, hardenability and size-dependent properties require separate verification. The standard includes hot-rolled wire rod; chemistry alone is no cold-heading supply commitment. Note 2: small composition deviations, excluding P/S, may be agreed when ordering restricted hardenability bands or quenched-and-tempered/normalized properties, but may not exceed Table 3. These data retain the Table 2 baseline without automatic relaxation. Light-typeface grades in note 4 are for special applications only. Note 5 permits separate ordering of Pb 0.15–0.30% only for the marked C-series grades; not added to ordinary base compositions. Original material number 1.7036; not marked for special application under note 4.

Verification notes

March 1987, Table 2 and all footnotes transcribed; mechanical properties checked separately.

28CrS4 · DIN EN 10084-2008

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10084-2008
Table / clause
Table 3, notes a–d

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.4283Known-element contribution; incomplete value; missing Cu, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3450–0.4600Known-element contribution; incomplete value; missing Mo, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.24 ~ 0.31
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.04
Cr0.9 ~ 1.2

Applicability and limitations

Ladle analysis, mass fraction wt%; the DIN EN 10084:2008-06 cover expressly identifies the German edition of EN 10084:2008; Table 3 follows that source text. Note b: minor composition deviations associated with hardenability requirements must be checked separately against Table 4 and the applicable conditions; they do not widen default ranges, and no such relaxation applies to P/S. Note c: higher S (approximately up to 0.10%) or Pb may be requested for improved machinability; in the higher-S case, the Mn upper limit may increase by 0.15 percentage points. Actual agreed values are not given; do not invent them or apply them automatically. Note d: B in this table improves toughness in the hardened case, not hardenability. Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); unspecified does not mean zero. A delivery standard for case-hardening steel does not mean all conditions are suitable for cold heading; verify mechanical properties, hardness and hardenability separately.

Verification notes

Original German Table 3 and its footnotes checked

Jominy end-quench hardenability (conditional requirements)

EN 10084:2008 · DIN EN 10084:2008-06, cover explicitly states German version of EN 10084:2008 · Table 5/Table 6/Table 8/Table 9; 7.1.2 and 8.2.2 · PDF pages 7, 10, 12, 18, 19, 22, 23

+H Normal hardenability band (7.1.2; applies to alloy steels in this standard unless otherwise agreed)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54553
34352
53951
72949
92545
112242
132039
15Unspecified; do not treat as 036
20Unspecified; do not treat as 033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HH Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54853
34652
54351
73649
93245
112942
132639
152336
202033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HL Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54550
34349
53947
72942
92538
112235
132033
15Unspecified; do not treat as 030
20Unspecified; do not treat as 027
25Unspecified; do not treat as 024
30Unspecified; do not treat as 023
35Unspecified; do not treat as 022
40Unspecified; do not treat as 021

28CrS4 · EN 10084-2008

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10084-2008
Table / clause
Table 3, notes a–d

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.4283Known-element contribution; incomplete value; missing Cu, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3450–0.4600Known-element contribution; incomplete value; missing Mo, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.24 ~ 0.31
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.04
Cr0.9 ~ 1.2

Applicability and limitations

Ladle analysis, mass fraction wt%; the DIN EN 10084:2008-06 cover expressly identifies the German edition of EN 10084:2008; Table 3 follows that source text. Note b: minor composition deviations associated with hardenability requirements must be checked separately against Table 4 and the applicable conditions; they do not widen default ranges, and no such relaxation applies to P/S. Note c: higher S (approximately up to 0.10%) or Pb may be requested for improved machinability; in the higher-S case, the Mn upper limit may increase by 0.15 percentage points. Actual agreed values are not given; do not invent them or apply them automatically. Note d: B in this table improves toughness in the hardened case, not hardenability. Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); unspecified does not mean zero. A delivery standard for case-hardening steel does not mean all conditions are suitable for cold heading; verify mechanical properties, hardness and hardenability separately.

Verification notes

The official German edition of DIN expressly adopts EN10084:2008; Table 3 and footnotes have been checked

Jominy end-quench hardenability (conditional requirements)

EN 10084:2008 · DIN EN 10084:2008-06, cover explicitly states German version of EN 10084:2008 · Table 5/Table 6/Table 8/Table 9; 7.1.2 and 8.2.2 · PDF pages 7, 10, 12, 18, 19, 22, 23

+H Normal hardenability band (7.1.2; applies to alloy steels in this standard unless otherwise agreed)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54553
34352
53951
72949
92545
112242
132039
15Unspecified; do not treat as 036
20Unspecified; do not treat as 033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HH Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54853
34652
54351
73649
93245
112942
132639
152336
202033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HL Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54550
34349
53947
72942
92538
112235
132033
15Unspecified; do not treat as 030
20Unspecified; do not treat as 027
25Unspecified; do not treat as 024
30Unspecified; do not treat as 023
35Unspecified; do not treat as 022
40Unspecified; do not treat as 021

28CrS4 · NF EN 10084-2008

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Adopted-standard basis verified
Standard edition
EN 10084-2008
Table / clause
Table 3, notes a–d

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.4283Known-element contribution; incomplete value; missing Cu, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3450–0.4600Known-element contribution; incomplete value; missing Mo, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.24 ~ 0.31
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.04
Cr0.9 ~ 1.2

Applicability and limitations

Ladle analysis, mass fraction wt%; the DIN EN 10084:2008-06 cover expressly identifies the German edition of EN 10084:2008; Table 3 follows that source text. Note b: minor composition deviations associated with hardenability requirements must be checked separately against Table 4 and the applicable conditions; they do not widen default ranges, and no such relaxation applies to P/S. Note c: higher S (approximately up to 0.10%) or Pb may be requested for improved machinability; in the higher-S case, the Mn upper limit may increase by 0.15 percentage points. Actual agreed values are not given; do not invent them or apply them automatically. Note d: B in this table improves toughness in the hardened case, not hardenability. Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); unspecified does not mean zero. A delivery standard for case-hardening steel does not mean all conditions are suitable for cold heading; verify mechanical properties, hardness and hardenability separately.

Verification notes

The official adoption relationship for NF and original EN10084:2008, Table 3 have been checked; The complete main text of NF has not been checked page by page

Jominy end-quench hardenability (conditional requirements)

EN 10084:2008 · DIN EN 10084:2008-06, cover explicitly states German version of EN 10084:2008 · Table 5/Table 6/Table 8/Table 9; 7.1.2 and 8.2.2 · PDF pages 7, 10, 12, 18, 19, 22, 23

+H Normal hardenability band (7.1.2; applies to alloy steels in this standard unless otherwise agreed)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54553
34352
53951
72949
92545
112242
132039
15Unspecified; do not treat as 036
20Unspecified; do not treat as 033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HH Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54853
34652
54351
73649
93245
112942
132639
152336
202033
25Unspecified; do not treat as 030
30Unspecified; do not treat as 029
35Unspecified; do not treat as 028
40Unspecified; do not treat as 027

+HL Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 850 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54550
34349
53947
72942
92538
112235
132033
15Unspecified; do not treat as 030
20Unspecified; do not treat as 027
25Unspecified; do not treat as 024
30Unspecified; do not treat as 023
35Unspecified; do not treat as 022
40Unspecified; do not treat as 021

28CrS4 · DIN 17200-1987

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN 17200-1987-03
Table / clause
Table 2 and footnotes 1–5; 7.3.1–7.3.2
PDF page references
1、2、15、16、17

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3150–0.4283Known-element contribution; incomplete value; missing Cu, Ni, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3450–0.4600Known-element contribution; incomplete value; missing Mo, Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.24 ~ 0.31
Mn0.6 ~ 0.9
S0.02 ~ 0.035
Cr0.9 ~ 1.2
Si≤ 0.4 (lower limit not stated)
P≤ 0.035 (lower limit not stated)

Applicability and limitations

Table 2 cast analysis, mass fraction wt%; Si is an upper limit and unspecified elements are not filled with zero. P/S requirements for the C, Ck and Cm series remain separate; S 0.020–0.035% in S-containing grades is a two-sided range. Note 1: unlisted elements may not be intentionally added without purchaser consent, except to complete melting; no fixed residual values are inferred. Table 3 contains permissible product-analysis deviations, not added to cast limits; applicable sizes and positive/negative directions are checked separately. Heat-treatment condition, hardenability and size-dependent properties require separate verification. The standard includes hot-rolled wire rod; chemistry alone is no cold-heading supply commitment. Note 2: small composition deviations, excluding P/S, may be agreed when ordering restricted hardenability bands or quenched-and-tempered/normalized properties, but may not exceed Table 3. These data retain the Table 2 baseline without automatic relaxation. Light-typeface grades in note 4 are for special applications only. Note 5 permits separate ordering of Pb 0.15–0.30% only for the marked C-series grades; not added to ordinary base compositions. Original material number 1.7036; not marked for special application under note 4.

Verification notes

March 1987, Table 2 and all footnotes transcribed; mechanical properties checked separately.

28CrS4 · DIN EN ISO 683-3-2019

Original-source verification is incomplete; this is not a formal standard reference

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.24 ~ 0.31
Cr0.9 ~ 1.2
Cu≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.04
Si≤ 0.4 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.

28CrS4 · ISO 683-3-2019

Original-source verification is incomplete; this is not a formal standard reference

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Verification status
Reference data; original source not verified

Carbon-equivalent reference

IIW / CEV: composition source not verified; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): composition source not verified; standard-range carbon equivalent is not calculated
CET: composition source not verified; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
C0.24 ~ 0.31
Cr0.9 ~ 1.2
Cu≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S0.02 ~ 0.04
Si≤ 0.4 (lower limit not stated)

Applicability and limitations

A match in the materials database does not establish suitability for cold heading or guarantee finished-product strength. Confirmation must consider wire condition, deformation, heat treatment and tests on actual parts.