← BackMaterial grade directory

25CRMO4

14 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 25CRMO4 →

25CrMo4 · EN 10263

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Drawn wire
Original record status
Reference transcription of standard
Standard edition
BS EN 10263-4:2017
Table / clause
Table 3

Carbon-equivalent reference

IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

Heat analysis; see the source page for footnotes and agreement-based options. An unspecified range is not zero. The early temporary 2001 extraction has been replaced with the 2017 original. The website does not state an edition; this entry shows the edition of its source and does not establish contractual applicability.

Verification notes

Standard source: BS EN 10263-4:2017 · Table 3View associated products →

25CrMo4 · ISO 4954

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Cold-heading wire
Original record status
Reference transcription of standard
Standard edition
ISO 4954:2018
Table / clause
Table C.2

Carbon-equivalent reference

IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

ISO 4954:2018; heat analysis, mass fraction %; values without a stated range are upper limits; see the source page for complete table footnotes. The website does not specify the edition; the source edition is shown here and does not establish contractual applicability.

Verification notes

Standard source: ISO 4954:2018 · Table C.2View associated products →

25CrMo4 · ISO 4954-2018

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Steel for quenching and tempering
Material form
Reference record
Original record status
Original standard verified
Standard edition
ISO 4954:2018
Table / clause
Table C.2

Carbon-equivalent reference

IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

ISO 4954:2018, Table C.2 gives heat analysis; A single value is a maximum; a dash is not zero. ; Product-analysis tolerances are listed separately under Table 2/3 of the standard and do not directly widen the heat-analysis composition ranges. ; Optional Al0.020–0.050% to improve cold-heading performance; this is not a universal mandatory minimum. ; Low Si may be agreed in the order, taking hardenability into account; Where hardenability is required, the standard permits limited deviations, except for P/S; C must not exceed 0.01%; see Table 2 for the other requirements. ; For C, a range of width 0.04% may be agreed; it does not replace the tabulated range by default.

Verification notes

Table C.2 and its footnotes in the standard text were checked.

25CrMo4 · EN 10263-4-2017

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10263-4-2017
Table / clause
Table 3 and notes

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default heat composition listed in the table; optional Al addition not selected.
IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.
IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3

Applicability and limitations

EN10263-4:2017, Table 3, heat analysis, mass percent. ; Elements not listed shall not be filled as 0; they shall not be intentionally added without the consent of the purchaser, except additions needed to finish steelmaking. ; Note 2 allows the specification of small deviations when hardenability requirements exist, but this does not involve P/S; The default composition range is not expanded here; it must be combined with specific hardenability ordering conditions. ; Note 3 allows Al 0.020–0.050% to be listed separately; it shall not be defaulted as mandatory aluminum content. ; Mechanical properties and delivery conditions are to be verified separately; the standard range is not a guarantee for the forming of arbitrary parts. ; Note a: lower Si may be agreed upon, but the influence on properties such as hardenability must be considered; do not fill in if no specific agreement range is provided. ; Note b allows a C range of 0.04% width by agreement; the example .33–.37 is not a uniform range for all grades.

Original condition-branch records

Default heat composition listed in the table; optional Al addition not selected.

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3

Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Al0.02 ~ 0.05

A condition branch must be selected

Yes

Verification notes

Visual check of Tables 3 and 4 and footnotes in the English original

25CrMo4 · DIN EN 10263-4-2002

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10263-4-2002
Table / clause
Table 2

Carbon-equivalent reference

IIW / CEV:0.5300–0.7567Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4375Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4825Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.3 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3

Applicability and limitations

DIN EN10263-4:2002-02 adopts EN10263-4:2001; the edition relationship is expressly identified on the cover; Heat-analysis mass percentages. ; Historical Table 2/3 contains no optional Al addition note for 2017; newer-edition conditions are not applied. ; Table 2, note c permits an agreed carbon range of width .04%; tabulated defaults are unchanged without a specific agreement. ; Table 2, note d and Table 3, note c permit agreed lower Si, considering effects on properties/hardenability; no range is invented where none is specified. ; Unlisted elements are not entered as zero; Table 2, note a: intentional additions without purchaser consent are prohibited except to finish the heat; residuals may be present but must not impair properties. ; Table 2, note b permits specified deviations where hardenability is required, except for P/S; The default composition range is not widened here. ; Mechanical properties, delivery and hardenability require separate verification; suitability for forming a specific component requires separate confirmation.

Verification notes

Older-edition Tables 2 and 3 and footnotes visually checked; equivalence to the newer edition is not assumed.

25CrMo4 · DIN EN 10083-3-2007

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10083-3-2007
Table / clause
Table 3 · Notes a–c
PDF page references
1、18

Carbon-equivalent reference

IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Mn0.6 ~ 0.9
S≤ 0.035 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Si≤ 0.4 (lower limit not stated)
P≤ 0.025 (lower limit not stated)

Applicability and limitations

Composition is based on Table 3 of EN10083-3:2006 in the official English text of DIN EN10083-3:2007-01, heat analysis wt%. ; Note a: Elements not listed shall not be intentionally added without the purchaser's consent, except for additions needed to finish steelmaking and to enable boron to act on hardenability.; Unspecified values shall not be treated as zero. ; Note b: Small deviations are permitted where hardenability or quenched-and-tempered mechanical-property requirements apply, except for C/P/S; permitted deviations for other elements must not exceed Table 4.; Default heat analysis range shall not be expanded. ; For non-boron steels in this standard, Note c permits steel with improved machinability to be supplied on request: sulfur approximately 0.10%, with the Mn upper limit permitted to increase by an absolute 0.15%.; Approximate values are not default hard upper limits and must be determined by specific inquiry/order; they shall not be automatically mixed with ordinary grades. ; This standard covers alloy steels for quenching and tempering. Suitability for cold heading, wire-rod supply, annealing, surface and dimensions require separate confirmation; do not automatically add products..

Verification notes

Official English source cover, all 28 grades in Table 3 and notes a–c visually checked.

Permitted product-analysis deviations (must not be added to heat-analysis limits)

DIN EN10083-3:2007-01 (adopting EN10083-3:2006) · Table 4 and notes a/b, 7.1.2.2; Product analysis specified at ordering follows A.5 · PDF pages 11, 19, 55 · mass fraction wt%; Deviations are expressed in percentage points of mass percentage

The complete standard tolerance table applies only to elements specified in the original table for this grade and to the corresponding content/sulfur-range conditions; it does not widen heat-analysis composition, carbon equivalent or reverse-search ranges.

ElementSpecified maximum heat-analysis content, wt%Lower deviation, percentage pointsUpper deviation, percentage pointsApplicable conditions
C≤0.55-0.02+0.02Select the cast-analysis maximum-content band specified in the original table
Si≤0.40The original table does not state a negative deviation+0.03Select the cast-analysis maximum-content band specified in the original table
Mn≤1.00-0.04+0.04Select the cast-analysis maximum-content band specified in the original table
Mn>1.00≤1.70-0.05+0.05Select the cast-analysis maximum-content band specified in the original table
P≤0.025The original table does not state a negative deviation+0.005Select the cast-analysis maximum-content band specified in the original table
S≤0.040The original table does not state a negative deviation+0.005Only the sulfur upper limit is specified; Note b’s full 0.020–0.040% range is not applied.
Cr≤2.00-0.05+0.05Select the cast-analysis maximum-content band specified in the original table
Cr>2.00≤2.20-0.1+0.1Select the cast-analysis maximum-content band specified in the original table
Mo≤0.30-0.03+0.03Select the cast-analysis maximum-content band specified in the original table
Mo>0.30≤0.60-0.04+0.04Select the cast-analysis maximum-content band specified in the original table
Ni≤2.00-0.05+0.05Select the cast-analysis maximum-content band specified in the original table
Ni>2.00≤4.3-0.07+0.07Select the cast-analysis maximum-content band specified in the original table
V≤0.25-0.02+0.02Select the cast-analysis maximum-content band specified in the original table
B≤0.0050-0.0003+0.0003Select the cast-analysis maximum-content band specified in the original table
S≤0.040-0.005+0.005Only when Table 3 heat analysis explicitly specifies the full S range of 0.020–0.040% (Table 4, Note b).

This is a complete standard deviation table and does not imply that every element for this grade is specified; Elements not listed are not added on the basis of this table. Symmetric deviation for the same heat is permitted in only one direction, either upward or downward; Asymmetric deviation for Pb is only found in the Pb row of EN10087 and cannot be applied to other standards where Pb is not listed. Do not automatically expand heat analysis composition, carbon equivalent, or reverse-lookup ranges.

25CrMo4 · EN 10269-2013

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10269-2013
Table / clause
Table1 quenched-and-tempered steels and note a/b/c
PDF page references
17、19

Carbon-equivalent reference

IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3

Applicability and limitations

EN10269:2013 Table 1, section on steels for quenching and tempering; official BS adoption in English, PDF17 and footnotes PDF19; heat analysis wt%.. ; The Al column is total aluminum; For ≥.020 without a specified upper limit, only the lower limit is retained; no upper limit shall be created. ; Note b sulfur agreement applies only to grades with Note b; 27NiCrMoV15-6 magnetic properties Note c carbon upper limit .28 selected separately. ; Elements not listed shall not be intentionally added without the consent of the purchaser, except additions needed to finish steelmaking; Blank does not represent zero. ; Product analysis deviation, mechanical properties, heat treatment, and cold-heading supply suitability shall be verified separately, and not automatically added to the product center.

Verification notes

Quenched-and-tempered steels in official English Table 1 and the applicable footnotes were visually checked

25CrMo4 · DIN 17200-1987

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN 17200-1987-03
Table / clause
Table 2 and footnotes 1–5; 7.3.1–7.3.2
PDF page references
1、2、15、16、17

Carbon-equivalent reference

IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Mn0.6 ~ 0.9
S≤ 0.03 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3
Si≤ 0.4 (lower limit not stated)
P≤ 0.035 (lower limit not stated)

Applicability and limitations

Table 2 cast analysis, mass fraction wt%; Si is an upper limit and unspecified elements are not filled with zero. P/S requirements for the C, Ck and Cm series remain separate; S 0.020–0.035% in S-containing grades is a two-sided range. Note 1: unlisted elements may not be intentionally added without purchaser consent, except to complete melting; no fixed residual values are inferred. Table 3 contains permissible product-analysis deviations, not added to cast limits; applicable sizes and positive/negative directions are checked separately. Heat-treatment condition, hardenability and size-dependent properties require separate verification. The standard includes hot-rolled wire rod; chemistry alone is no cold-heading supply commitment. Note 2: small composition deviations, excluding P/S, may be agreed when ordering restricted hardenability bands or quenched-and-tempered/normalized properties, but may not exceed Table 3. These data retain the Table 2 baseline without automatic relaxation. Light-typeface grades in note 4 are for special applications only. Note 5 permits separate ordering of Pb 0.15–0.30% only for the marked C-series grades; not added to ordinary base compositions. Original material number 1.7218; not marked for special application under note 4.

Verification notes

March 1987, Table 2 and all footnotes transcribed; mechanical properties checked separately.

25CrMo4 · NF EN 10269:1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Reference record
Original record status
Original-standard record
Standard edition
NF EN 10269:1999
Table / clause
EN 10269:1999 Table 1 and footnotes 1 and 2
PDF page references
2、21、23

Carbon-equivalent reference

IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.22 ~ 0.29
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr0.9 ~ 1.2
Mo0.15 ~ 0.3

Applicability and limitations

The cover of NF EN 10269:1999 explicitly adopts EN 10269:1999; Preserve the correspondence between the French adoption version and the European version; do not label as other countries or new editions. ; Table 1 gives heat-analysis mass percentages; Single values in P and S columns are upper limits; other single values are parsed according to the inequality signs in the original table; Unspecified elements shall not be filled as zero. ; Applies to billets, bars and wire rod of steels and nickel alloys for fasteners with specified high- or low-temperature properties.; Cold heading and actual supply must be verified in conjunction with delivery condition, dimensions, and process. ; Table 1 Footnote 1: Elements not listed in the table shall not be intentionally added without the buyer's consent (except additions needed to finish steelmaking); Elements that affect properties must be prevented from being introduced via scrap steel, etc.. ; This record only verifies the heat analysis composition in Table 1; product analysis tolerances in Table 2 shall not be automatically added to the heat limits.

Combined limits

Combined-element limits

    25CrMo4 · EN 10250-3-1999

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material category
    Alloy steel
    Subcategory
    Alloy steel
    Material form
    Reference record
    Original record status
    Original standard verified
    Standard edition
    EN 10250-3-1999
    Table / clause
    Table1 and note 1/2; Clauses 1, 3.1 and 3.2
    PDF page references
    6、8、9

    Source document

    Carbon-equivalent reference

    IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
    Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
    CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

    Composition

    ElementComposition requirement
    C0.22 ~ 0.29
    Si≤ 0.4 (lower limit not stated)
    Mn0.6 ~ 0.9
    P≤ 0.035 (lower limit not stated)
    S≤ 0.035 (lower limit not stated)
    Cr0.9 ~ 1.2
    Mo0.15 ~ 0.3

    Applicability and limitations

    Based on the original Table 1 and footnotes of EN10250-3:1999 as recorded in BS EN10250-3:2000, heat analysis mass fraction is in wt%.. ; This standard covers alloy special-steel open-die forgings, forged bars and ring-rolled products after pre-forging, supplied in the quenched-and-tempered condition.; This does not automatically establish a supply standard for cold-heading wire.. ; Table 1 Note 1 allows the manufacturer to add Al, Ti, V, Nb individually or in combination to control grain size.; No new numerical ranges are provided; values cannot be filled as zero or have upper limits arbitrarily determined.. Elements not listed in Table 1/2 shall not be intentionally added without the consent of the purchaser (except additions needed to finish steelmaking).. ; 3.1 requires the heat analysis composition to be in accordance with Table 1 and references A.7/A.8 of EN10250-1.; Clause 3.2: Apply product-analysis tolerances separately under Table 2 and Clause 9.2 of EN10250-1; do not directly expand the default heat-analysis range.. ; Currently, only chemical compositions, grade/steel number correspondences, and related range footnotes are confirmed.; It is not declared that all mechanical properties and the referenced Part 1 have been verified..

    Verification notes

    Both pages, all 21 rows and footnotes of Table 1 were visually checked; Each element and its separate font mapping were restored and compared with the original table cells, with matching results

    25CrMo4 · EN 10132-3-2000

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material category
    Alloy steel
    Subcategory
    Alloy steel
    Material form
    Cold-rolled narrow strip; dimensions and delivery condition subject to applicable conditions
    Original record status
    Original standard verified
    Standard edition
    EN 10132-3:2000
    Table / clause
    Table 1; Table 2; clauses 1,4,7.3–7.5
    PDF page references
    1、4、5、8
    Unit
    Mass fraction (wt%)
    Analysis type
    Heat analysis

    Carbon-equivalent reference

    IIW / CEV:0.5300–0.7400Known-element contribution; incomplete value; missing V, Ni, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
    Pcm(Ito–Bessyo):0.3050–0.4283Known-element contribution; incomplete value; missing Cu, Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
    CET:0.3400–0.4700Known-element contribution; incomplete value; missing Cu, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

    Composition

    ElementComposition requirement
    C0.22 ~ 0.29
    Si≤ 0.4 (lower limit not stated)
    Mn0.6 ~ 0.9
    P≤ 0.035 (lower limit not stated)
    S≤ 0.035 (lower limit not stated)
    Cr0.9 ~ 1.2
    Mo0.15 ~ 0.3

    Applicability and limitations

    Actually based on the official English text of EN 10132-3:2000; This standard covers cold-rolled narrow steel strip intended for heat treatment; it does not constitute a supply guarantee for cold-heading wire.. Table 1 is for heat analysis; Permissible deviations for finished product analysis in Table 2 are registered independently; finished product permissible deviations shall not be used to relax heat analysis. Table 1 Footnote: Elements not listed shall not be intentionally added without the buyer's consent, except additions needed to finish steelmaking; Prevent scrap or other raw materials from introducing elements that could impair properties or intended use; unlisted elements must not be assumed zero.. Values in Mechanical Table 3 are applicable only for 0.30 mm≤t<3.00 mm; Mechanical properties for thicker steel strips shall be agreed upon during inquiry and ordering and cannot be directly extrapolated. Footnote a of Table 3 requires a choice between tensile indicators and hardness; Unless otherwise specified, tensile requirements apply. This page presents the alternatives separately and does not treat both as simultaneous guaranteed requirements.. For cold-rolled +CR, agree a tensile-property interval 150 MPa wide when tensile requirements are selected, or a hardness interval 50 HV wide when hardness is selected.; The outer boundaries of this table do not automatically generate actual ordering windows. Sampling, test methods, microstructure, dimensions, inspection, and other general delivery requirements shall also be verified in conjunction with EN10132-1 and applicable agreements; composition reverse-check does not replace full-item acceptance. This part covers cold-rolled narrow steel strip for quenching and tempering; strip supplied for heat treatment has thickness up to 6mm.; The +QT condition is within the range of 0.30 to 3.00mm, but the values in Table 3 are strictly limited to 0.30≤t<3.00mm.. +QT is used only for grades with explicitly listed values in Table 3.; The actual ordering range for tensile strength or hardness shall be agreed upon based on the 150MPa or 50HV width respectively; the entire optional interval in the table cannot be treated as a single supply guarantee.. +AC spheroidizing annealing condition may be adopted by agreement, but spheroidization and mechanical limits must be separately agreed upon.; +A/+LC values shall not be applied.. The +CR mechanical properties for 25Mn4 and CrMo grades must be agreed upon during ordering..

    Verification notes

    The complete original English Table 1 was transcribed; Table 2 product-analysis tolerances and Table 3 condition/thickness and alternative tensile-or-hardness requirements have been checked

    Permitted product-analysis deviations

    C
    Permitted deviation
    0.02
    Deviation direction
    Positive or negative deviation; only one direction is permitted for the same heat
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    Si
    Permitted deviation
    0.03
    Deviation direction
    Only positive deviations are permitted
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    Mn
    Permitted deviation
    0.04
    Deviation direction
    Positive or negative deviation; only one direction is permitted for the same heat
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    P
    Permitted deviation
    0.005
    Deviation direction
    Only positive deviations are permitted
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    S
    Permitted deviation
    0.005
    Deviation direction
    Only positive deviations are permitted
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    Cr
    Permitted deviation
    0.04
    Deviation direction
    Positive or negative deviation; only one direction is permitted for the same heat
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged
    Mo
    Permitted deviation
    0.03
    Deviation direction
    Positive or negative deviation; only one direction is permitted for the same heat
    Applicable conditions
    Product analysis; For the same heat, deviations may be above the upper limit or below the lower limit, but not both; Heat-analysis limits remain unchanged

    25CrMo4 · EN ISO 683-2-2018

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material category
    Alloy steel
    Subcategory
    Alloy steel for quenching and tempering
    Material form
    Reference record
    Original record status
    Original standard verified
    Standard edition
    EN ISO 683-2-2018
    Table / clause
    Table 3, notes a–d; clause 7.1.2; Table 4 limits
    PDF page references
    21
    Unit
    Mass fraction (wt%)
    Analysis type
    Heat analysis; not product analysis

    Carbon-equivalent reference

    IIW / CEV:0.5300–0.7667Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
    Pcm(Ito–Bessyo):0.3083–0.4483Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
    CET:0.3400–0.4900Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

    Composition

    ElementComposition requirement
    C0.22 ~ 0.29
    Si0.1 ~ 0.4
    Mn0.6 ~ 0.9
    P≤ 0.025 (lower limit not stated)
    S≤ 0.035 (lower limit not stated)
    Cu≤ 0.4 (lower limit not stated)
    Cr0.9 ~ 1.2
    Mo0.15 ~ 0.3

    Applicability and limitations

    Table 3 herein applies to heat (cast) analysis, mass fraction wt%; The permissible deviations for product analysis in Table 4 shall not be directly added to the limits in general Table 3. This document is EN ISO 683-2:2018, adopted without modification and accompanied by the text of ISO 683-2:2016; This record explicitly preserves the identity of EN ISO 683-2-2018 and shall not be called the ISO 2018 edition. Only the chemical composition and source conditions of Table 3 are verified; this does not constitute a guarantee of hardenability, heat treatment, mechanical properties, wire delivery state, or cold heading process. Note a: deviations in heat analysis apply only when hardenability requirements are specified; The deviation in C shall not exceed ±0.01%; P/S is excluded, and the other elements follow Table 4. General Table 3 shall not be automatically relaxed, nor shall H/HH/HL be merged with general grades. Note b: Steel with S increased to approximately 0.10% (including sulfide morphology control) or with the addition of Pb to improve machinability may be requested from the supplier; When S is increased, the upper limit of Mn may be increased by 0.15 percentage points. This agreement is not a default requirement, and approximate values shall not serve as precise automatic limits for this batch; if the Pb range is not listed, values shall not be borrowed from other standards. Original Note: Elements not listed shall not be intentionally added without the consent of the purchaser, except those required to complete the melting process; Elements introduced via scrap steel etc. shall be controlled. An unlisted value must not be assumed to be zero. Note d: lower Si is permitted, but other deoxidation methods must be used; The original text does not provide a uniform lower Si range; agreed conditions shall not automatically replace the range listed in 0.10–0.40%.

    Verification notes

    Original-image verification of all 25 physical rows and merged cells in Table 3; reuse existing independently cropped evidence for 5 same-source rows and 40 cells, transcribe the remaining cells individually from the source images, and record the two editions separately.

    25CrMo4 · ISO 683-2-2016

    Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

    Material category
    Alloy steel
    Subcategory
    Alloy steel for quenching and tempering
    Material form
    Reference record
    Original record status
    Original standard verified
    Standard edition
    ISO 683-2-2016
    Table / clause
    Table 3, notes a–d; clause 7.1.2; Table 4 limits
    PDF page references
    21
    Unit
    Mass fraction (wt%)
    Analysis type
    Heat analysis; not product analysis

    Carbon-equivalent reference

    IIW / CEV:0.5300–0.7667Known-element contribution; incomplete value; missing V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
    Pcm(Ito–Bessyo):0.3083–0.4483Known-element contribution; incomplete value; missing Ni, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
    CET:0.3400–0.4900Known-element contribution; incomplete value; missing Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

    Composition

    ElementComposition requirement
    C0.22 ~ 0.29
    Si0.1 ~ 0.4
    Mn0.6 ~ 0.9
    P≤ 0.025 (lower limit not stated)
    S≤ 0.035 (lower limit not stated)
    Cu≤ 0.4 (lower limit not stated)
    Cr0.9 ~ 1.2
    Mo0.15 ~ 0.3

    Applicability and limitations

    Table 3 herein applies to heat (cast) analysis, mass fraction wt%; The permissible deviations for product analysis in Table 4 shall not be directly added to the limits in general Table 3. This document is EN ISO 683-2:2018, adopted without modification and accompanied by the text of ISO 683-2:2016; This record explicitly preserves the identity of ISO 683-2-2016 and shall not be called the ISO 2018 edition. Only the chemical composition and source conditions of Table 3 are verified; this does not constitute a guarantee of hardenability, heat treatment, mechanical properties, wire delivery state, or cold heading process. Note a: deviations in heat analysis apply only when hardenability requirements are specified; The deviation in C shall not exceed ±0.01%; P/S is excluded, and the other elements follow Table 4. General Table 3 shall not be automatically relaxed, nor shall H/HH/HL be merged with general grades. Note b: Steel with S increased to approximately 0.10% (including sulfide morphology control) or with the addition of Pb to improve machinability may be requested from the supplier; When S is increased, the upper limit of Mn may be increased by 0.15 percentage points. This agreement is not a default requirement, and approximate values shall not serve as precise automatic limits for this batch; if the Pb range is not listed, values shall not be borrowed from other standards. Original Note: Elements not listed shall not be intentionally added without the consent of the purchaser, except those required to complete the melting process; Elements introduced via scrap steel etc. shall be controlled. An unlisted value must not be assumed to be zero. Note d: lower Si is permitted, but other deoxidation methods must be used; The original text does not provide a uniform lower Si range; agreed conditions shall not automatically replace the range listed in 0.10–0.40%.

    Verification notes

    Original-image verification of all 25 physical rows and merged cells in Table 3; reuse existing independently cropped evidence for 5 same-source rows and 40 cells, transcribe the remaining cells individually from the source images, and record the two editions separately.

    25CrMo4 · DIN EN 10277:2018-09

    Original table in an informative annex verified; normative composition requirements and edition still require verification. For reference only.

    Material category
    Alloy steel
    Subcategory
    Alloy steel
    Material form
    Reference record
    Composition basis
    Heat analysis in an informative annex; for reference only
    Verification status
    Original table in an informative annex verified; normative composition requirements and edition still require verification
    Standard edition
    DIN EN 10277:2018-09
    Table / clause
    Informative Annex A.4
    PDF page references
    47
    Unit
    mass fraction (wt%)
    Analysis type
    Heat analysis (informative reference)

    Carbon-equivalent reference

    Composition from an informative standard annex is for reference only. Normative composition and edition remain unverified; standard-range carbon equivalents and reverse matching are disabled.

    Composition

    ElementComposition requirement
    C0.22 ~ 0.29
    Si0.1 ~ 0.4
    Mn0.6 ~ 0.9
    P≤ 0.025 (lower limit not stated)
    S≤ 0.035 (lower limit not stated)
    Cr0.9 ~ 1.2
    Mo0.15 ~ 0.3
    Cu≤ 0.4 (lower limit not stated)

    Applicability and limitations

    The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.

    Composition conditions

    Conditional requirement

    Verification notes

    The original informative-annex table has been checked and is for reference only. Clause 7.1.2 requires chemical composition to be determined under the cited standard; the formal normative composition and applicable edition remain unverified. Do not use it as a delivery guarantee, a reverse-search acceptance criterion or a basis for standard-range carbon equivalent.
    WhatsApp Technical enquiry →