← BackMaterial grade directory

23MNB4

7 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 23MNB4 →

23MnB4 · EN 10263

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Drawn wire
Original record status
Reference transcription of standard
Standard edition
BS EN 10263-4:2017
Table / clause
Table 4

Carbon-equivalent reference

IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
B0.0008 ~ 0.005

Applicability and limitations

Heat analysis; see the source page for footnotes and agreement-based options. An unspecified range is not zero. The early temporary 2001 extraction has been replaced with the 2017 original. The website does not state an edition; this entry shows the edition of its source and does not establish contractual applicability.

Verification notes

Standard source: BS EN 10263-4:2017 · Table 4View associated products →

23MnB4 · ISO 4954

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Cold-heading wire
Original record status
Reference transcription of standard
Standard edition
ISO 4954:2018
Table / clause
Table C.3

Carbon-equivalent reference

IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
B0.0008 ~ 0.005
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

ISO 4954:2018; heat analysis, mass fraction %; values without a stated range are upper limits; see the source page for complete table footnotes. The website does not specify the edition; the source edition is shown here and does not establish contractual applicability.

Verification notes

Standard source: ISO 4954:2018 · Table C.3View associated products →

23MnB4 · ISO 4954-2018

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Steel for quenching and tempering
Material form
Reference record
Original record status
Original standard verified
Standard edition
ISO 4954:2018
Table / clause
Table C.3

Carbon-equivalent reference

IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
B0.0008 ~ 0.005
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

ISO 4954:2018, Table C.3 gives heat analysis; A single value is a maximum; a dash is not zero. ; Product-analysis tolerances are listed separately under Table 2/3 of the standard and do not directly widen the heat-analysis composition ranges. ; Optional Al0.020–0.050% to improve cold-heading performance; this is not a universal mandatory minimum. ; Low Si may be agreed in the order, taking hardenability into account; Where hardenability is required, the standard permits limited deviations, except for P/S; C must not exceed 0.01%; see Table 2 for the other requirements. ; When a Cr maximum of 0.30% is specified, a minimum Cr may be agreed at ordering; 30MoB1 requires guaranteed hardenability, with Cr minimum 0.15% and an upper limit adjustable by agreement.

Verification notes

The original standard, Table C.3 and footnotes have been checked

23MnB4 · EN 10263-4-2017

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10263-4-2017
Table / clause
Table 4 and notes

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default heat composition listed in the table; optional Al addition not selected.
IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.
IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
B0.0008 ~ 0.005

Applicability and limitations

EN10263-4:2017, Table 4, heat analysis, mass percent. ; Elements not listed shall not be filled as 0; they shall not be intentionally added without the consent of the purchaser, except additions needed to finish steelmaking. ; Note 2 allows the specification of small deviations when hardenability requirements exist, but this does not involve P/S; The default composition range is not expanded here; it must be combined with specific hardenability ordering conditions. ; Note 3 allows Al 0.020–0.050% to be listed separately; it shall not be defaulted as mandatory aluminum content. ; Mechanical properties and delivery conditions are to be verified separately; the standard range is not a guarantee for the forming of arbitrary parts. ; The text of Table 4 Note a indicates that a Cr lower limit may be agreed upon for grades with Cr≤.30%; the table header Footnote a is located at Si; the ambiguity of the original position is retained, and clear Si table values shall not be changed nor low Si conditions arbitrarily set based on this. ; The Cr lower limit of .15 in Table 4 Note b applies only to the core hardenability requirements of 1.5408 (30MoB1) and shall not be applied to other grades such as 30MnB4; Agreement to reduce the Cr upper limit must include a specific limit value.

Original condition-branch records

Default heat composition listed in the table; optional Al addition not selected.

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
B0.0008 ~ 0.005

Note 3: optional Al addition of 0.020–0.050% to improve cold-heading performance.

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
B0.0008 ~ 0.005
Al0.02 ~ 0.05

A condition branch must be selected

Yes

Verification notes

Visual check of Tables 3 and 4 and footnotes in the English original

23MnB4 · DIN EN 10263-4-2002

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10263-4-2002
Table / clause
Table 3

Carbon-equivalent reference

IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)
B0.0008 ~ 0.005

Applicability and limitations

DIN EN10263-4:2002-02 adopts EN10263-4:2001; the edition relationship is expressly identified on the cover; Heat-analysis mass percentages. ; Historical Table 2/3 contains no optional Al addition note for 2017; newer-edition conditions are not applied. ; Table 2, note c permits an agreed carbon range of width .04%; tabulated defaults are unchanged without a specific agreement. ; Table 2, note d and Table 3, note c permit agreed lower Si, considering effects on properties/hardenability; no range is invented where none is specified. ; Unlisted elements are not entered as zero; Table 2, note a: intentional additions without purchaser consent are prohibited except to finish the heat; residuals may be present but must not impair properties. ; Table 2, note b permits specified deviations where hardenability is required, except for P/S; The default composition range is not widened here. ; Mechanical properties, delivery and hardenability require separate verification; suitability for forming a specific component requires separate confirmation. ; Historical Table 3, note d: minima for grades with Cr≤.30 may be agreed, but no general value is given; the 30MoB1 core-hardening .15 option from 2017 is not copied.

Verification notes

Older-edition Tables 2 and 3 and footnotes visually checked; equivalence to the newer edition is not assumed.

23MnB4 · EN 10269-2013

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
EN 10269-2013
Table / clause
Table1 quenched-and-tempered steels and note a/b/c
PDF page references
17、19

Carbon-equivalent reference

IIW / CEV:0.3500–0.5267Known-element contribution; incomplete value; missing Mo, V, Ni CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3725Known-element contribution; incomplete value; missing Ni, Mo, V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.3975Known-element contribution; incomplete value; missing Mo, Ni CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Al≥ 0.02 (upper limit not stated)
B0.0008 ~ 0.005
Cr≤ 0.3 (lower limit not stated)
Cu≤ 0.25 (lower limit not stated)

Applicability and limitations

EN10269:2013 Table 1, section on steels for quenching and tempering; official BS adoption in English, PDF17 and footnotes PDF19; heat analysis wt%.. ; The Al column is total aluminum; For ≥.020 without a specified upper limit, only the lower limit is retained; no upper limit shall be created. ; Note b sulfur agreement applies only to grades with Note b; 27NiCrMoV15-6 magnetic properties Note c carbon upper limit .28 selected separately. ; Elements not listed shall not be intentionally added without the consent of the purchaser, except additions needed to finish steelmaking; Blank does not represent zero. ; Product analysis deviation, mechanical properties, heat treatment, and cold-heading supply suitability shall be verified separately, and not automatically added to the product center.

Verification notes

Quenched-and-tempered steels in official English Table 1 and the applicable footnotes were visually checked

23MnB4 · BEXG 021-2020

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
BEXG 021-2020, sixteenth revision stated on the cover; issued and effective on 2020-12-29; The latest original document available on this computer only
Document title
Technical delivery conditions for cold-heading steel wire rod for automotive parts
Table / clause
Table 1
PDF page references
6
Unit
Mass fraction (wt%)
Manufacturer
Baoshan Iron & Steel Co., Ltd. (Baosteel)

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.3500–0.5520Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2490–0.3798Known-element contribution; incomplete value; missing V Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2900–0.4085 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.2 ~ 0.25
Si≤ 0.3 (lower limit not stated)
Mn0.9 ~ 1.2
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr≤ 0.3 (lower limit not stated)
B0.0008 ~ 0.005
Cu≤ 0.25 (lower limit not stated)
Ni≤ 0.2 (lower limit not stated)
Mo≤ 0.06 (lower limit not stated)

Applicability and limitations

Baosteel BEXG 021-2020, Table 1, row 54, PDF page 6; heat-analysis composition in wt%, hot-rolled wire rod. 2020 is the original edition available locally, with no claim that it is the company’s current latest edition. Special conditions and actual supply require separate confirmation.

Composition conditions

Verification notes

Table 1 original images checked page by page, physical pages 3–10; continuation values and other columns kept separate; two disputed rows excluded.

Source footnotes

B:0.0008-0.0050,Cu≤0.25
WhatsApp Technical enquiry →