18NiCr5-4 · DIN EN 10084-2008

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
DIN EN 10084-2008
Table / clause
Table 3, notes a–d

Carbon-equivalent reference

IIW / CEV:0.5200–0.7000Known-element contribution; incomplete value; missing Mo, V, Cu CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2550–0.3533Known-element contribution; incomplete value; missing Cu, Mo, V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2950–0.3975Known-element contribution; incomplete value; missing Mo, Cu CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.16 ~ 0.21
Si≤ 0.4 (lower limit not stated)
Mn0.6 ~ 0.9
P≤ 0.025 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cr0.9 ~ 1.2
Ni1.2 ~ 1.5

Applicability and limitations

Ladle analysis, mass fraction wt%; the DIN EN 10084:2008-06 cover expressly identifies the German edition of EN 10084:2008; Table 3 follows that source text. Note b: minor composition deviations associated with hardenability requirements must be checked separately against Table 4 and the applicable conditions; they do not widen default ranges, and no such relaxation applies to P/S. Note c: higher S (approximately up to 0.10%) or Pb may be requested for improved machinability; in the higher-S case, the Mn upper limit may increase by 0.15 percentage points. Actual agreed values are not given; do not invent them or apply them automatically. Note d: B in this table improves toughness in the hardened case, not hardenability. Unlisted elements must not be intentionally added without purchaser approval (except as necessary during steelmaking); unspecified does not mean zero. A delivery standard for case-hardening steel does not mean all conditions are suitable for cold heading; verify mechanical properties, hardness and hardenability separately.

Verification notes

Original German Table 3 and its footnotes checked

Jominy end-quench hardenability (conditional requirements)

EN 10084:2008 · DIN EN 10084:2008-06, cover explicitly states German version of EN 10084:2008 · Table 5/Table 6/Table 8/Table 9; 7.1.2 and 8.2.2 · PDF pages 7, 10, 12, 18, 20, 22, 23

+H Normal hardenability band (7.1.2; applies to alloy steels in this standard unless otherwise agreed)

End-quench test temperature 880 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54149
33948
53546
73244
92942
112739
132537
152436
202134
252032
30Unspecified; do not treat as 031
35Unspecified; do not treat as 031
40Unspecified; do not treat as 030

+HH Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 880 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54449
34248
53946
73644
93342
113139
132937
152836
202534
252432
302331
352331
402230

+HL Restricted hardenability band (Table 6; agreement at enquiry and order required)

End-quench test temperature 880 °C (tolerance not stated in the source); this is not a production heat-treatment recommendation.

Distance from quenched end (mm)Lower limit (HRC)Upper limit (HRC)
1.54146
33945
53542
73240
92938
112735
132533
152432
202130
252028
30Unspecified; do not treat as 027
35Unspecified; do not treat as 027
40Unspecified; do not treat as 026