← BackMaterial grade directory

15CRMO

5 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 15CRMO →

15CrMo · GB/T 3077-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy structural steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 3077-2015
Table / clause
Tables 1 and 2; A/E designation rules in the endnote to Table 1

Carbon-equivalent reference

IIW / CEV:0.4267–0.6667Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3390Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3825 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.12 ~ 0.18
Mn0.4 ~ 0.7
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
Si0.17 ~ 0.37
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)

Applicability and limitations

GB/T 3077-2015 Table 1 gives ladle analysis; Table 2 gives P/S and residual-element requirements. The final note to Table 1 allows ordering any grade as higher or special quality by adding A or E after the grade; this record is ordinary quality steel. For steel used in hot-pressure working, Cu ≤0.20%; the ordinary Cu maximum does not apply to this use. Explicit alloy ranges in Table 1 take priority; for Cr/Ni/Mo not specified there, use the residual limits in Table 2 and do not add residual limits on top of alloying-element ranges. Sn/Sb/As must be analyzed and recorded on the inspection certificate; any needed limits require agreement, and no generic numerical limits are invented here. Product-analysis deviations are handled separately under GB/T 222 and do not directly expand ladle limits. Mechanical properties depend on specimen dimensions and the recommended heat-treatment/delivery condition; this composition review does not constitute verification of properties.

Verification notes

Tables 1/2 and quality-grade rules checked

15CrMo · Q/BQB 517-2023

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Cold-heading steel
Material form
Hot-rolled steel wire rod for cold heading
Original record status
Original standard verified
Standard edition
Q/BQB 517—2023
Table / clause
6.1.1/Table 1, row 81, note a
PDF page references
11
Unit
Mass fraction (wt%)
Analysis type
Heat analysis

Source document

Carbon-equivalent reference

IIW / CEV:0.4267–0.6533Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3323Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3750 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.12 ~ 0.18
Si0.17 ~ 0.37
Mn0.4 ~ 0.7
P≤ 0.02 (lower limit not stated)
S≤ 0.02 (lower limit not stated)
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)

Applicability and limitations

Q/BQB 517—2023, official original on the Baosteel website, Table 1, row 81; cast-analysis mass fraction wt%. Table footnote a: residual Cr≤0.20, Ni≤0.20, Cu≤0.20, Mo≤0.06 wt%; where this row specifies otherwise, its requirement for that element takes precedence. Unlisted elements and special agreement requirements must not be treated as zero or assumed guarantees; permitted product-analysis deviations are governed separately by GB/T 222. Wire rod is delivered hot rolled; stricter P/S under Z1 and special surface or inclusion quality must be confirmed under normative Annex A and the contractual ordering codes. Fixed mechanical properties must not be inferred from the chemistry table.

Verification notes

All 104 rows of Table 1 and 34 rows of Table 2 in the original Q/BQB517:2023 from Baosteel’s official website were checked row by row; not mixed with older editions.View associated products →

15CrMo · GB/T 3078-2019

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy structural steel
Material form
Cold-drawn bars
Original record status
Original standard verified
Standard edition
GB/T 3078-2019

Carbon-equivalent reference

IIW / CEV:0.4267–0.6667Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3390Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3825 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.12 ~ 0.18
Mn0.4 ~ 0.7
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
Si0.17 ~ 0.37
P≤ 0.03 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)

Applicability and limitations

Clause 7.1.1 of GB/T3078—2019: quality carbon structural steels comply with GB/T699, and alloy structural steels with GB/T3077; the referenced composition standard must also be displayed. This grade is listed in row 45 of Table 2. Hardness for each delivery condition is listed separately under Table 2; the actual application and delivery condition require separate verification and are not assumed to comply. Cold-drawn steel bars/cold-drawn polished round bars: product-analysis deviations under GB/T222 require separate verification and are not added to heat-analysis ranges. In GB/T3077-2015, Table 1 gives heat analysis and Table 2 gives P/S and residual-element requirements. The final note to Table 1 permits all grades to be ordered as higher or special quality, with the respective suffixes A/E; this record uses the default quality-steel class. Steel for hot pressure working: Cu≤0.20%; the ordinary Cu upper limit does not apply to that use. Explicit alloy ranges in Table 1 take precedence. Where Cr/Ni/Mo is not explicitly specified, the residual limits in Table 2 apply; residual limits are not added to specified alloy-element ranges. Sn/Sb/As must be analysed and recorded on the inspection certificate, with limits agreed where needed; no universal numerical limit is invented here. Product-analysis deviations under GB/T222 are used separately and do not directly widen heat-analysis ranges. Mechanical properties depend on specimen dimensions and the recommended heat-treatment/delivery conditions; this composition review does not establish verification of mechanical properties.

Verification notes

GB/T 3078-2019 Table 2 grade rows and the clause 7.1.1 reference checked; composition comes from the verified GB/T 3077-2015 original, not a separate composition table in GB/T 3078.

Hardness in the delivery condition (conditions shown separately)

GB/T 3078-2019 · Table 2 hardness in delivery condition and Note a; 7.3/7.4 · PDF pages 6, 7 · HBW

Standard condition data, not actual measured results of supplied heats; Actual delivery condition, application, and contract must be confirmed.

Cold-drawn or cold-drawn and bright-polished delivery; Table 2 conditions are for general use. For hot-pressure-working applications, check clause 7.4.2 separately.

HBW:≤ 229 (lower limit not stated) HBW

Delivery in the annealed, bright-annealed, high-temperature-tempered or tempered-after-normalizing condition; delivery as-normalized is excluded and shall be agreed by both parties under 7.4.1.

HBW:≤ 187 (lower limit not stated) HBW

15CrMo · BEXG 021-2020

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Cold-heading steel
Subcategory
Cold-heading steel
Material form
Wire rod
Original record status
Manufacturer source verified
Document edition
BEXG 021-2020, sixteenth revision stated on the cover; issued and effective on 2020-12-29; The latest original document available on this computer only
Document title
Technical delivery conditions for cold-heading steel wire rod for automotive parts
Table / clause
Table 1
PDF page references
3
Unit
Mass fraction (wt%)
Manufacturer
Baoshan Iron & Steel Co., Ltd. (Baosteel)

Carbon-equivalent reference

Estimate from manufacturer-published ranges, not a standard guarantee or measured heat result; formula applicability requires review against the application and process.

IIW / CEV:0.4267–0.6533Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3323Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3750 Envelope of independent element limits from manufacturer data; neither standard guarantee values nor measured heat results CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition

ElementComposition requirement
C0.12 ~ 0.18
Si0.17 ~ 0.37
Mn0.4 ~ 0.7
P≤ 0.025 (lower limit not stated)
S≤ 0.025 (lower limit not stated)
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
Ni≤ 0.2 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)

Applicability and limitations

Baosteel BEXG 021-2020, Table 1, row 5, PDF page 3; heat-analysis composition in wt%, hot-rolled wire rod. 2020 is the original edition available locally, with no claim that it is the company’s current latest edition. Special conditions and actual supply require separate confirmation.

Composition conditions

Verification notes

Table 1 original images checked page by page, physical pages 3–10; continuation values and other columns kept separate; two disputed rows excluded.

Source footnotes

Mo:0.40-0.55View associated products →

15CrMo · GB/T 3077-1999

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy structural steel
Material form
Reference record
Original record status
Original standard verified
Standard edition
GB/T 3077-1999
Table / clause
Table 1, No. 35 and notes 1–4; Table 2; 6.1.1–6.1.2
PDF page references
5、7、8
Unit
Mass fraction (wt%)
Analysis type
Heat analysis, not product analysis

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Quality steel; machining or other non-hot-pressure processing: Cu limit per Table 2.
IIW / CEV:0.4267–0.6667Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3390Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3825 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.
Quality steel; hot-pressure working, clause 6.1.1.3: Cu ≤0.20%.
IIW / CEV:0.4267–0.6600Known-element contribution; incomplete value; missing V CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; an engineering estimate of welding cold-cracking susceptibility for carbon and low-alloy steels.
Pcm(Ito–Bessyo):0.2123–0.3340Known-element contribution; incomplete value; missing V, B Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B; mainly used for low-carbon low-alloy steels, particularly modern low-carbon pipeline steels; more relevant when C is approximately no higher than 0.11%.
CET:0.2400–0.3775 Independent-element envelope of standard ranges; not measured heat-analysis values CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40; used in welding preheat assessment for ferritic steels, subject to the applicability conditions of EN 1011-2.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.12 ~ 0.18
Si0.17 ~ 0.37
Mn0.4 ~ 0.7
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)

Applicability and limitations

GB/T 3077—1999, Table 1: ladle analysis, mass fraction wt%; this record follows the actual 1999 edition, not the 2015 edition. Grades without suffix A in the table are ordered as quality steel. Table 2 P/S/Cu and residual Mo follow the applicable quality grade; residual Cr/Ni/Mo limits do not override alloy contents specified in Table 1. The chemical composition also applies to ingots, billets and their products; bar scope, mechanical properties and surface-quality requirements do not by themselves guarantee suitability as cold-heading wire. If the processing use is not specified in the contract, machining applies; for hot-pressure processing, Cu≤0.20%, select the applicable condition. Under 6.1.1.2, residual W/V/Ti are analyzed and reported on the certificate; no common limit is stated for unlisted elements, so do not enter zero; Table 1 alloy ranges for W/V/Ti remain applicable. Table 1 Note 2: upgrading to A/E quality or specifying other chemistry by agreement requires a separate order check; do not merge grades or rewrite this row’s C range. Note 4: rare earth 0.05% is a calculated addition; product analysis is for reference, not a guaranteed range. Product-analysis tolerances for steel/billets are separately checked against cited GB/T 222—1984 and do not automatically relax ladle limits.

Original condition-branch records

Quality steel; machining or other non-hot-pressure processing: Cu limit per Table 2.

ElementComposition requirement
C0.12 ~ 0.18
Si0.17 ~ 0.37
Mn0.4 ~ 0.7
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)

Quality steel; hot-pressure working, clause 6.1.1.3: Cu ≤0.20%.

ElementComposition requirement
C0.12 ~ 0.18
Si0.17 ~ 0.37
Mn0.4 ~ 0.7
Cr0.8 ~ 1.1
Mo0.4 ~ 0.55
P≤ 0.035 (lower limit not stated)
S≤ 0.035 (lower limit not stated)
Cu≤ 0.2 (lower limit not stated)
Ni≤ 0.3 (lower limit not stated)

A condition branch must be selected

Yes

Verification notes

The 1999 original images of Tables 1 and 2 and the related clauses were checked. Heat analysis, quality grade and hot-working conditions are retained as separate conditions.