← BackMaterial grade directory

1100

3 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 1100 →

1100 · GB/T 3190—1996

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Aluminum and aluminum alloys
Subcategory
Aluminum and aluminum alloys
Material form
Reference record
Original record status
Original-standard record
Standard edition
GB/T 3190—1996
Table / clause
Table 1; Clause 4.1~4.5 · Footnotes
PDF page references
3、5、13

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
Cu0.05 ~ 0.2
Mn≤ 0.05 (lower limit not stated)
Zn≤ 0.1 (lower limit not stated)
Al≥ 99.0 (upper limit not stated)

Applicability and limitations

GB/T 3190—1996, Table 1, mass percent; Unspecified elements are not treated as zero. ; This standard covers chemical composition of wrought aluminum and aluminum alloys; This does not establish cold-heading suitability, actual supply or finished-product properties. ; Al is listed as a minimum content; Aluminum content is calculated by difference under Clause 4.1/4.2, using the specified inclusion thresholds and precision; unmeasured elements must not be treated as zero. ; Individual and combined limits for other impurities concern only the other elements defined in Clause 4.3 of the standard, not the sum of all principal alloying elements; Missing impurity test results must not be treated as zero. ; Table 1, footnote 1: for welding electrodes and surfacing applications, beryllium content must not exceed 0.0008%.

Combined limits

Combined-element limits
  • Requirement
    Si+Fe (GB/T 3190—1996, Table 1)
    Element coefficient
    Si
    1
    Fe
    1
    Lower limit
    Not stated
    Upper limit
    0.95
Elements requiring measured values from the same heat
  • Fe
  • Si
Purity calculation rules in the source
PDF page references
3
Purity from 99.00% to below 99.90%
Al = 100 minus the sum of all other elements present at ≥0.010%; before summing, express each element to 0.0X%.
Purity from 99.90% to 99.99%
Al = 100 minus the sum of all other elements present at ≥0.001%; before summing, express each element to 0.00X%, then round the result to 0.0X%.
Rounding rules
Follow GB/T 8170; do not treat unspecified elements as zero or apply ordinary remainder calculations directly.
Purity requires technical review
Yes
Other-impurity requirements in the source
Each other impurity
0.05
Sum of other impurities
0.15
Other impurities require technical review
Yes
Conditional requirements in the source
  • Footnote
    1
    Source conditions
    For welding electrodes and surfacing applications, beryllium content must not exceed 0.0008%.
    Automatic evaluation implemented
    No

1100 · JIS H 4040-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS H 4040:2015
Table / clause
Table 1: applicable product forms and designations; Table 2: chemical composition and footnotes.
PDF page references
15
Unit
Mass fraction (%)
Analysis type
Chemical composition (refer to the source notes for the analysis type)

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
Cu0.05 ~ 0.2
Mn≤ 0.05 (lower limit not stated)
Zn≤ 0.1 (lower limit not stated)
Al≥ 99.0 (upper limit not stated)

Applicability and limitations

Table 2 coupled limit: Si+Fe≤0.95%; a combined maximum is not treated as an independent maximum for each element. ; Table 2, footnote b: Be≤0.0003% applies only to filler rods and welding wire; it is not a default restriction for all forms. ; Each otherwise unlisted element is ≤0.05%; this is not automatically treated as a known limit for a specific element. ; The combined total of otherwise unlisted elements is ≤0.15%. ; Table 1 applicable forms: extruded bars, cold-drawn bars and cold-drawn wire; Form codes correspond only to Table 1 of this edition and do not establish supply by Creation Group. ; Table 2 gives chemical composition in mass percent; Mechanical properties, dimensions and delivery condition require separate verification against the applicable original tables and order requirements.

Verification notes

2015: Tables 1 and 2 in the original English edition corrected page by page and cell by cell; alloy designation 1100; original PDF page 15, Table 2

1100 · JIS H 4040-2006

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material form
Reference record
Original record status
Original standard verified
Standard edition
JIS H 4040:2006
Table / clause
Table 1: applicable product forms and designations; Table 2: chemical composition and footnotes.
PDF page references
8
Unit
Mass fraction (%)
Analysis type
Chemical composition (refer to the source notes for the analysis type)

Carbon-equivalent reference

IIW / CEV: not directly applicable to this material category
Pcm (Ito–Bessyo): not directly applicable to this material category
CET: not directly applicable to this material category

Composition

ElementComposition requirement
Cu0.05 ~ 0.2
Mn≤ 0.05 (lower limit not stated)
Zn≤ 0.1 (lower limit not stated)
Al≥ 99.0 (upper limit not stated)

Applicability and limitations

Table 2 coupled limit: Si+Fe≤0.95%; a combined maximum is not treated as an independent maximum for each element. ; Table 2, footnote 2: Be≤0.0003% applies only to filler rods and welding wire; it is not a default restriction for all forms. ; Each otherwise unlisted element is ≤0.05%; this is not automatically treated as a known limit for a specific element. ; The combined total of otherwise unlisted elements is ≤0.15%. ; Table 1 applicable forms: extruded bars, cold-drawn bars and cold-drawn wire; Form codes correspond only to Table 1 of this edition and do not establish supply by Creation Group. ; Table 2 gives chemical composition in mass percent; Mechanical properties, dimensions and delivery condition require separate verification against the applicable original tables and order requirements.

Verification notes

2006: Tables 1 and 2 in the original Japanese edition corrected page by page and cell by cell; alloy designation 1100; original PDF page 8, Table 2