102Cr6 material reference
3 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.
Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.
Open condition selection, comparison and carbon-equivalent tools for 102CR6 →102Cr6 · ISO 4957-2018
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Reference record
- Original record status
- Original standard verified
- Standard edition
- ISO 4957-2018
- Table / clause
- Table 4 · Notes a–g
- PDF page references
- 15、16
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.95 ~ 1.1 |
| Si | 0.15 ~ 0.35 |
| Mn | 0.25 ~ 0.45 |
| Cr | 1.35 ~ 1.65 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Applicability and limitations
Table 4 heat composition for cold-work alloy tool steels, wt%; Default P/S are each ≤.030%. ; Product-analysis tolerances in Table 5 must not be applied to the default heat-analysis range. ; Unlisted elements must not be intentionally added without purchaser consent, except additions needed to finish steelmaking; dashes are not entered as zero. ; Cold-work tool steel does not establish suitability for cold-heading wire; the words “cold work” alone do not justify listing a product in the product centre.
Verification notes
Official English Table 4 and footnotes visually checked.102Cr6 · DIN EN 10132-4-2000(+AC:2002)
Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results
- Material form
- Narrow strip only
- Original record status
- Original standard verified
- Standard edition
- DIN EN 10132-4-2000(+AC:2002)
- Table / clause
- Analysis-type boundaries in Table 1 and note a, and Table 2
- PDF page references
- 1、6
Carbon-equivalent reference
Composition
| Element | Composition requirement |
|---|---|
| C | 0.95 ~ 1.1 |
| Si | 0.15 ~ 0.35 |
| Mn | 0.2 ~ 0.4 |
| Cr | 1.35 ~ 1.6 |
| Ni | ≤ 0.4 (lower limit not stated) |
| P | ≤ 0.025 (lower limit not stated) |
| S | ≤ 0.025 (lower limit not stated) |
| Mo | ≤ 0.1 (lower limit not stated) |
Applicability and limitations
Official German DIN 2003-04 adopts EN10132-4:2000+AC:2002; PDF6, Table 1 gives heat-analysis mass fractions wt%. ; Cold-rolled narrow strip for heat-treatment applications; Covers spring steels and other special applications; it does not establish a basis for supply as cold-heading wire rod. ; Product-analysis tolerances in Table 2 are listed separately and are not mixed with the default heat-analysis range in Table 1; Within the same heat, ±tolerances must not be exceeded in both the lower and upper directions. ; Elements not listed in the table must not be intentionally added without purchaser consent, except to finish steelmaking; unspecified contents are not treated as zero. ; AC:2002 corrects the annealed/lightly skin-passed properties in Table 3; Only the complete Table 1 chemical composition was checked in this batch; mechanical properties require separate verification.
Verification notes
All 15 rows and footnotes in the official original text were visually checked102Cr6 · BS EN ISO 4957:2018
Chemical-composition source verified. Properties and delivery conditions follow the sources and conditions stated here; actual supply and measured heat results are not verified by this reference.
- Material category
- Tool steel
- Product form
- Tool-steel standard reference; product form subject to the order
- Standard edition
- BS EN ISO 4957:2018
- Table / clause
- Table 4 and notes a–g
- Source file
- BS EN ISO 4957-2018-Tool steel.docx
- Units
- Mass fraction (wt%)
- Analysis type
- Cast analysis
Composition
| Element | Composition requirement |
|---|---|
| C | 0.95 ~ 1.1 |
| Si | 0.15 ~ 0.35 |
| Mn | 0.25 ~ 0.45 |
| Cr | 1.35 ~ 1.65 |
| P | ≤ 0.03 (lower limit not stated) |
| S | ≤ 0.03 (lower limit not stated) |
Applicability and limitations
Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero. Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking. Permissible product-analysis deviations do not expand the default cast-analysis limits. Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition. Table 4: alloy cold-work tool steels; cast analysis, wt%; default P and S each ≤.030%. Product-analysis deviations in Table 5 must not be applied to the default cast-analysis limits. Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Dashes are not entered as zero. Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Composition and ordering conditions
- Cast analysis, mass fraction %. A dash means the standard gives no separate requirement; it does not mean zero.
- Unlisted elements shall not be intentionally added without purchaser consent, except additions needed to finish steelmaking.
- Permissible product-analysis deviations do not expand the default cast-analysis limits.
- Tool-steel classification and hardness depend on application, heat treatment and test conditions; they do not establish cold-heading suitability or guarantee properties in an arbitrary condition.
- Table 4: alloy cold-work tool steels; cast analysis, wt%; default P and S each ≤.030%.
- Product-analysis deviations in Table 5 must not be applied to the default cast-analysis limits.
- Unlisted elements shall not be intentionally added without purchaser consent, except to finish steelmaking. Dashes are not entered as zero.
- Annealed and cold-drawn (+A+C) hardness may be 20 HBW higher than annealed (+A) hardness. Hardness values for different conditions must not be interchanged.
Mechanical properties and delivery condition
| Property | Standard requirements and applicable conditions |
|---|---|
| Annealed hardness HBW / maximum | 223 |
| Hardening test | Austenitizing 840±10 °C ; oil quenching ; tempering 180±10 °C ; hardness≥60 HRC |
Mechanical-property provenance:BS EN ISO 4957:2018 · Table 4 and notes a–g · Standard tables embedded in the Word document supplied by the user
Verification notes
Checked against the standard text and table notes supplied by the user. Applicability to a specific order requires separate confirmation.